Poly(allyl diglycol carbonate), ADC (CR-39) ADC (CR-39)
Poly(allyl diglycol carbonate), a crosslinked thermoset of the monomer diethylene glycol bis(allyl carbonate), C12H18O7 (monomer) · CAS 25656-90-0 for the polymer (Wikipedia infobox); 142-22-3 for the monomer (Wikipedia infobox)
Poly(allyl diglycol carbonate), sold as CR-39, is a clear, rigid thermoset made by polymerising the liquid monomer allyl diglycol carbonate (C12H18O7).
Evidence level
5 of 5
Flown or field-proven
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Let light through
91 % light transmittance
Bend light well
1.498 refractive index
Detect particles
3 % energy resolution for 2.9 MeV protons
Stay clear in heat
100 °C continuous use
Recipe, share of the weight
- ADC Molar mass 274.2700 g/mol (NASA Table IV)Diethylene glycol bis(allyl carbonate), allyl diglycol carbonate
- IPP Share not readDiisopropyl peroxydicarbonate
Best for
Light, clear optical parts and track detectors: 1.498 refractive index and about half the weight of glass (Wikipedia)
Weakest at
Atomic oxygen in low Earth orbit (erosion yield above 6.80e-24 cm3/atom on MISSE 2) and UV, which changes its optical absorption and etch behaviour
Risk at a glance
- People Low. Monomer hazardous, polymer not classified
- If it fails Severe. Atomic oxygen erosion in low Earth orbit
- Corrosion Severe. The erosion yield is above 6.80e-24 cm3/atom, so the sample eroded through before the end of the exposure.
Quick facts: ADC (CR-39)
| Property | Value | Basis |
|---|---|---|
| Density | 1.14 to 1.32 g/cm³ | 3 sourced values across conditions |
| Thermal expansion (CTE) | 117 ppm/K | 1 sourced value |
| Melting point | -4 °C | 1 sourced value |
| Maximum service temperature | 100 °C | 1 sourced value |
What is the density of Poly, ADC (CR-39)?
Poly, ADC (CR-39) has a density of 1.14 to 1.32 g/cm³. The range covers 3 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the coefficient of thermal expansion of Poly, ADC (CR-39)?
Poly, ADC (CR-39) has a coefficient of thermal expansion of 117 ppm/K. The source and test conditions are listed in the properties table on this page.
What is the melting point of Poly, ADC (CR-39)?
Poly, ADC (CR-39) has a melting point of -4 °C. The source and test conditions are listed in the properties table on this page.
What is the maximum service temperature of Poly, ADC (CR-39)?
Poly, ADC (CR-39) has a maximum service temperature of 100 °C. The source and test conditions are listed in the properties table on this page.
What is Poly, ADC (CR-39) used for?
Uses recorded in the sources include Eyeglass and sunglass lenses; Solid-state nuclear track detector (dosimetry, not shielding); Space exposure test sample (MISSE 2, flight).
Why it exists
CR-39 is a clear, light plastic: its refractive index is 1.498, its specific gravity is 1.32 and it transmits 91 % of light in the patent comparison. Its heat resistance is 91 °C, and it weighs about half as much as glass. It is also a reliable track detector, with energy resolution of 3 % for 2.9 MeV protons.
Where it's used
Eyeglass lenses
CR-39 lenses weigh about half as much as glass, and the first were made in 1947.
Track detectors
CR-39 records alpha particles, neutrons, protons and radon, and is etched in sodium hydroxide to reveal tracks.
Space test
ADC (CR-39) flew on the MISSE 2 PEACE tray on the ISS from 2001 to 2005, with an erosion yield greater than 6.80e-24 cm3/atom.
Recipe
Poly(allyl diglycol carbonate), a crosslinked thermoset of the monomer diethylene glycol bis(allyl carbonate), C12H18O7 (monomer)
Poly(allyl diglycol carbonate) is made by polymerising the liquid monomer diethylene glycol bis(allyl carbonate), C12H18O7 (NASA Table IV; Wikipedia). The monomer is cured with a peroxide initiator, diisopropyl peroxydicarbonate, over about 18 hours (patent Table 1). The allyl groups crosslink, which makes the polymer a thermoset with no melting point.
| Ingredient | Share of the weight | What it does |
|---|---|---|
| Diethylene glycol bis(allyl carbonate), allyl diglycol carbonate ADC | Molar mass 274.2700 g/mol (NASA Table IV) | Monomer. Its allyl groups crosslink on polymerisation. |
| Diisopropyl peroxydicarbonate IPP | Share not read | Initiator for the radical cure. Benzoyl peroxide is an alternative that gives a higher yellowness index (Wikipedia). |
Weight shares are as printed in the sources.
What it can do
Let light through
91 % light transmittance
measured
The CR-39 comparative example in the patent transmits 91 % of light, and a commercial 2 mm ADC plate transmits 92 %.
Bend light well
1.498 refractive index
measured
The cured plastic has a refractive index of 1.498, close to the value for crown glass, per Wikipedia.
Detect particles
3 % energy resolution for 2.9 MeV protons
measured
The track-detector study reports 3 % energy resolution for 2.9 MeV protons and 4 % for 3.15 MeV.
Stay clear in heat
100 °C continuous use
measured
CR-39 is rated for continuous use up to 100 °C, and up to one hour at 130 °C per Wikipedia (citation needed).
How it compares
The patent comparison puts CR-39 at 91 % light transmittance and a 1.498 refractive index. These are single comparative examples, so they are examples rather than a ranking against other optical plastics.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | ADC (CR-39) | PC |
|---|---|---|
| Capacity and energy | ||
| Energy resolution, 2.9 MeV protons | 3 %16 | no data |
| Thermal behavior and safety | ||
| Melting point, monomer ADCPrinted in the Wikipedia infobox for the monomer | -4 °C | no data |
| Physical and electrical | ||
| Density, cured polymer (MISSE 2 study table) | 1.317 g/cm³1 | 1190 kg/m3 |
| Specific gravity, CR-39 comparative example | 1.32 specific gravity (unitless)2 | 1190 kg/m3 |
| Density, liquid monomer ADC | 1.143 g/cm³3 | 1190 kg/m3 |
| Temperature behavior | ||
| Heat resistance, equal to the glass transition per the source | 91 °C8 | 144 °C |
| Other measurements | ||
| Refractive index, cured CR-39 | 1.498 unitless4 | 1.59 dimensionless |
| Refractive index, monomer ADC | 1.45 unitless5 | 1.59 dimensionless |
| Light transmittance, CR-39 comparative example | 91 %6 | 89 % |
| Light transmittance, commercial ADC plates | 92 %7 | 89 % |
| Continuous use temperature | 100 °C9 | no data |
| Linear expansion coefficient, CR-39 comparative example | 117 µm/m/°C10 | no data |
| Water absorption, CR-39 comparative example | 0.2 %11 | no data |
| Atomic oxygen erosion yield, MISSE 2 (lower bound) | > 6.8×10^-24 cm³/atom12 | 4.29×10^-24 cm³/atom |
| Atomic oxygen erosion yield, predicted | 6.3×10^-24 cm³/atom13 | 4.29×10^-24 cm³/atom |
| Molar mass, repeat unit C12H18O7Printed in the NASA erosion study Table IV | 274.3 g/mol | no data |
| Optical absorption coefficient, UV-C band (215-242 nm) | 54 cm-114 | no data |
| Optical absorption coefficient, UV-A band (315-400 nm) | 1 cm-115 | no data |
| Polymerization time, CR-39 comparative examplePrinted in a patent comparative example table | 18 hours | no data |
Why choose it, and why not
Good for
- Light optical parts: 1.498 refractive index and 91 % light transmittance in the patent comparison.
- Track detection: 3 % energy resolution for 2.9 MeV protons in the track-detector study.
- Weight: about half the weight of glass for eyeglass lenses (Wikipedia).
Watch out for
- Atomic oxygen: the MISSE 2 sample eroded through, with an erosion yield greater than 6.80e-24 cm3/atom.
- UV at 254 nm: optical absorption reaches 54 cm-1 in the 215-242 nm band, and etch behaviour changes.
- Monomer hazards: H302, H315 and H410 apply to the liquid monomer, and the cured polymer was not classified.
CR-39 is a clear, light thermoset with 1.498 refractive index, 91 % light transmittance and 100 °C continuous use, which suits eyeglass lenses and track detection. It is weak in low Earth orbit, where the MISSE 2 sample eroded through, and under short-wavelength UV.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Density, cured polymer (MISSE 2 study table) | Value printed in the NASA erosion study, Table II, column g/cm3 | state cured polymertemperature not printed | — |
| 2 | Specific gravity, CR-39 comparative example | Printed in a patent comparative example table (specific gravity, no unit printed) | state cured polymertemperature not printed | — |
| 3 | Density, liquid monomer ADC | Value printed in the Wikipedia infobox for diallyl diglycol carbonate | state liquid monomer, allyl diglycol carbonatetemperature not printed | — |
| 4 | Refractive index, cured CR-39 | Printed as n_D in a patent comparative example and in Wikipedia | wavelength not printedstate cured polymer | — |
| 5 | Refractive index, monomer ADC | Printed as nD in the Wikipedia infobox for the monomer | state liquid monomertemperature not printed | — |
| 6 | Light transmittance, CR-39 comparative example | Printed as "Transparence" in a patent comparative example table | thickness not printedstate cured polymer | — |
| 7 | Light transmittance, commercial ADC plates | Printed in a patent table for commercial ADC plates | thickness 2 mm platesstate commercial cured ADC | — |
| 8 | Heat resistance, equal to the glass transition per the source | Printed as heat resistance in a patent table; the text defines it as the temperature of maximum tan delta, which the patent calls Tg | basis temperature of maximum tan delta, which the source calls the glass transitionsample commercial ADC 2 mm plate | — |
| 9 | Continuous use temperature | Printed in the Wikipedia article for CR-39 (citation needed on the short-term figure) | duration continuousbasis optical use in eyeglasses | — |
| 10 | Linear expansion coefficient, CR-39 comparative example | Printed in a patent comparative example table as linear expansion coefficient | temperature range not printedstate cured polymer | — |
| 11 | Water absorption, CR-39 comparative example | Printed as water absorption rate in a patent comparative example table | duration not printedstate cured polymer | — |
| 12 | Atomic oxygen erosion yield, MISSE 2 (lower bound) | Flight measurement reported in the NASA predictive-tool report | bound lower bound; the printed value is greater than 6.80e-24 because the sample eroded throughexposure MISSE 2 PEACE tray on the ISS | — |
| 13 | Atomic oxygen erosion yield, predicted | Predicted value from the NASA predictive tool, compared with MISSE 2 in Table VII | exposure low Earth orbit atomic oxygen (predictive tool) | — |
| 14 | Optical absorption coefficient, UV-C band (215-242 nm) | Maximum value computed from UV-Vis spectra in the cited study | wavelength 215-242 nmexposure UV-exposed CR-39 | — |
| 15 | Optical absorption coefficient, UV-A band (315-400 nm) | Value computed from UV-Vis spectra in the cited study | wavelength 315-400 nmexposure UV-exposed CR-39 | — |
| 16 | Energy resolution, 2.9 MeV protons | Printed in the track-detector study, energy resolution section | particle protons, 2.9 MeVdetector 1 mm slotted CR-39 plate | — |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| UV light (wavelength 254 nm and 365 nm, laboratory lamp) | moderate | UV at 254 nm changes CR-39 optical absorption and its etch rate; UV at 365 nm did not change them in the cited study.1 |
| Atomic oxygen in low Earth orbit (MISSE 2, ISS, 3.95 years) | severe | The erosion yield is above 6.80e-24 cm3/atom, so the sample eroded through before the end of the exposure.2 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | UV light (wavelength 254 nm and 365 nm, laboratory lamp) | At 254 nm the UV-Vis spectrum shows blue and red shifts and the band gap decreases with exposure time. At 365 nm there was no significant change in bulk etch rate or UV-Vis spectrum, even after 80 hours. The study also found that the bulk etch rate is modified by a factor that depends on the UV dose. | exposure UV lamp 254 nm and 365 nm, 4 watt, samples 4 cm2etchant 6.25N NaOH at 70 °C |
| 2 | Atomic oxygen in low Earth orbit (MISSE 2, ISS, 3.95 years) | The lower-bound erosion yield exceeds the predicted value of 6.30e-24 cm3/atom, so the true yield is at least as high as the measured lower bound. | exposure MISSE 2 PEACE tray, ISS, outside the Quest airlock, 2001 to 2005 |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
The monomer carries H302, H315 and H410 hazard statements. The cured polymer was not classified in the pages read.
- Liquid monomer
- Diallyl diglycol carbonate has GHS statements H302, H315 and H410 with signal word Warning (Wikipedia).
If it fails
UV and atomic oxygen both change the material, and the MISSE 2 sample eroded through.
- UV at 254 nm
- UV at 254 nm raises optical absorption to 54 cm-1 in the 215-242 nm band, while UV-A at 315-400 nm gives only 1 cm-1 (Section 2).
- Atomic oxygen in orbit
- The MISSE 2 erosion yield is greater than 6.80e-24 cm3/atom after 3.95 years on the ISS, so the true yield is at least that.
Handling and storage
- Keep under the heat limit
- Continuous use is up to 100 °C for optics (Wikipedia).
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| UV-induced change in optical absorption and etch behaviourmoderate severity | Exposure to short-wavelength UV (254 nm in the cited study)Optical absorption rises and etch behaviour changes, so calibration of the track detector can drift. Changes at 365 nm were not measurable in the study. |
| Atomic oxygen erosion in low Earth orbitcritical severity | Long exposure to atomic oxygen on the ISS, MISSE 2 PEACE trayThe sample eroded through in the MISSE 2 flight, so its erosion yield is only a lower bound. |
Handling and storage
- Keep continuous use at or below 100 °C, since the Wikipedia article gives 130 °C only for up to one hour and marks it as citation needed.
- Handle the liquid monomer with the GHS precautions printed for it (H302, H315, H410); the cured polymer was not classified in the pages read.
Supply and geography
How common the raw materials are and where they come from.
Diethylene glycol bis(allyl carbonate) monomer (ADC)
- Top producers
- United States
CR-39 track detectors (sold to researchers)
- Top producers
- United Kingdom, United States, Japan
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: adc-cr-39
spore_version: 0.2
family: engineering-polymers
name: Poly(allyl diglycol carbonate), ADC (CR-39)
abbreviation: ADC (CR-39)
role: clear, light thermoset used for eyeglass lenses and as a solid-state nuclear track detector
category: polymers
type: polycarbonates
summary: Poly(allyl diglycol carbonate), sold as CR-39, is a clear, rigid thermoset made by polymerising the liquid monomer allyl diglycol carbonate (C12H18O7). The cured plastic has a refractive index of 1.498, a specific gravity of 1.32 and transmits 91 % of light in a comparative test. It is used for eyeglass lenses and as a track detector for alpha particles and neutrons. On MISSE 2 it flew on the ISS PEACE tray and its atomic-oxygen erosion yield was greater than 6.80e-24 cm3/atom.
best_for: 'Light, clear optical parts and track detectors: 1.498 refractive index and about half the weight of glass (Wikipedia)'
weakest_at: Atomic oxygen in low Earth orbit (erosion yield above 6.80e-24 cm3/atom on MISSE 2) and UV, which changes its optical absorption and etch behaviour
identity:
formula: Poly(allyl diglycol carbonate), a crosslinked thermoset of the monomer diethylene glycol bis(allyl carbonate), C12H18O7 (monomer)
cas: 25656-90-0 for the polymer (Wikipedia infobox); 142-22-3 for the monomer (Wikipedia infobox)
source: nasa-tm2008
where: Table IV, row ADC (CR-39), repeat unit C12H18O7 and molar mass 274.2700
tags:
environments:
- low-earth-orbit
stresses:
- atomic-oxygen
- uv
applications:
- optics-and-cameras
- radiation-shielding
properties:
- benchmark: density
label: Density, cured polymer (MISSE 2 study table)
value: 1.3173
unit: g/cm3
scope: material
conditions:
state: cured polymer
temperature: not printed
method: Value printed in the NASA erosion study, Table II, column g/cm3
status: ground
source: nasa-tm2008
where: Table II, row Allyl diglycol carbonate, ADC (CR-39)
- benchmark: density
label: Specific gravity, CR-39 comparative example
value: 1.32
unit: specific gravity (unitless)
scope: material
conditions:
state: cured polymer
temperature: not printed
method: Printed in a patent comparative example table (specific gravity, no unit printed)
status: ground
source: patent-us5350822
where: Table 1 and Table 3, CR-39 column (labelled Comparative Example 2)
- benchmark: density
label: Density, liquid monomer ADC
value: 1.143
unit: g/cm3
scope: material
conditions:
state: liquid monomer, allyl diglycol carbonate
temperature: not printed
method: Value printed in the Wikipedia infobox for diallyl diglycol carbonate
status: ground
source: wikipedia-adc
where: Infobox, Diallyl diglycol carbonate (ADC monomer)
- benchmark: refractive_index
label: Refractive index, cured CR-39
value: 1.498
unit: unitless
scope: material
conditions:
wavelength: not printed
state: cured polymer
method: Printed as n_D in a patent comparative example and in Wikipedia
status: ground
source: patent-us5350822
where: Table 1, CR-39 column; also Wikipedia CR-39 lead section
- benchmark: refractive_index
label: Refractive index, monomer ADC
value: 1.45
unit: unitless
scope: material
conditions:
state: liquid monomer
temperature: not printed
method: Printed as nD in the Wikipedia infobox for the monomer
status: ground
source: wikipedia-adc
where: Infobox, Diallyl diglycol carbonate (ADC monomer)
- benchmark: light_transmittance
label: Light transmittance, CR-39 comparative example
value: 91
unit: '%'
scope: material
conditions:
thickness: not printed
state: cured polymer
method: Printed as "Transparence" in a patent comparative example table
status: ground
source: patent-us5350822
where: Table 1, CR-39 column (labelled Comparative Example 2)
- benchmark: light_transmittance
label: Light transmittance, commercial ADC plates
value: 92
unit: '%'
scope: material
conditions:
thickness: 2 mm plates
state: commercial cured ADC
method: Printed in a patent table for commercial ADC plates
status: ground
source: patent-us6417273
where: Table 4, Comparative Example 1 (ADC, commercial 2 mm plates), light transmittance row
- benchmark: glass_transition_temperature
label: Heat resistance, equal to the glass transition per the source
value: 91
unit: °C
scope: material
conditions:
basis: temperature of maximum tan delta, which the source calls the glass transition
sample: commercial ADC 2 mm plate
method: Printed as heat resistance in a patent table; the text defines it as the temperature of maximum tan delta, which the patent calls Tg
status: ground
source: patent-us6417273
where: Table 4, Comparative Example 1, heat resistance row
- benchmark: max_service_temp
label: Continuous use temperature
value: 100
unit: °C
scope: material
conditions:
duration: continuous
basis: optical use in eyeglasses
method: Printed in the Wikipedia article for CR-39 (citation needed on the short-term figure)
status: ground
source: wikipedia-cr39
where: Applications, Optics section
- benchmark: cte
label: Linear expansion coefficient, CR-39 comparative example
value: 117
unit: µm/m/°C
scope: material
conditions:
temperature_range: not printed
state: cured polymer
method: Printed in a patent comparative example table as linear expansion coefficient
status: ground
source: patent-us5350822
where: Table 3, CR-39 row (Comparative Example 2)
- benchmark: moisture_absorption
label: Water absorption, CR-39 comparative example
value: 0.2
unit: '%'
scope: material
conditions:
duration: not printed
state: cured polymer
method: Printed as water absorption rate in a patent comparative example table
status: ground
source: patent-us5350822
where: Table 1, CR-39 column (Comparative Example 2)
- benchmark: atomic_oxygen_erosion_yield
label: Atomic oxygen erosion yield, MISSE 2 (lower bound)
value: 6.8e-24
unit: cm3/atom
bound: lower
scope: material
conditions:
bound: lower bound; the printed value is greater than 6.80e-24 because the sample eroded through
exposure: MISSE 2 PEACE tray on the ISS
method: Flight measurement reported in the NASA predictive-tool report
status: flight
source: nasa-tm2008
where: Table I, row Allyl diglycol carbonate, ADC (CR-39), MISSE 2 erosion yield column
- benchmark: atomic_oxygen_erosion_yield
label: Atomic oxygen erosion yield, predicted
value: 6.3e-24
unit: cm3/atom
scope: material
conditions:
exposure: low Earth orbit atomic oxygen (predictive tool)
method: Predicted value from the NASA predictive tool, compared with MISSE 2 in Table VII
status: calculated
source: nasa-tm2008
where: Table VII, row Allyl diglycol carbonate, predicted erosion yield column
- benchmark: molar_mass
label: Molar mass, repeat unit C12H18O7
value: 274.27
unit: g/mol
scope: material
conditions:
basis: repeat unit as tabulated by NASA
method: Printed in the NASA erosion study Table IV
status: ground
source: nasa-tm2008
where: Table IV, row Allyl diglycol carbonate, ADC (CR-39), molar mass column
- benchmark: melting_point
label: Melting point, monomer ADC
value: -4
unit: °C
scope: material
conditions:
state: liquid monomer
method: Printed in the Wikipedia infobox for the monomer
status: ground
source: wikipedia-adc
where: Infobox, Diallyl diglycol carbonate (ADC monomer)
- benchmark: optical_absorption_coefficient
label: Optical absorption coefficient, UV-C band (215-242 nm)
value: 54
unit: cm-1
scope: material
conditions:
wavelength: 215-242 nm
exposure: UV-exposed CR-39
method: Maximum value computed from UV-Vis spectra in the cited study
status: ground
source: inoe-uv-padc
where: Section 2 (Eq. 5 discussion), sentence on maximum optical absorption coefficient
- benchmark: optical_absorption_coefficient
label: Optical absorption coefficient, UV-A band (315-400 nm)
value: 1
unit: cm-1
scope: material
conditions:
wavelength: 315-400 nm
exposure: UV-exposed CR-39
method: Value computed from UV-Vis spectra in the cited study
status: ground
source: inoe-uv-padc
where: Section 2 (Eq. 5 discussion), same sentence as the 215-242 nm value
- benchmark: energy_resolution
label: Energy resolution, 2.9 MeV protons
value: 3
unit: '%'
scope: material
conditions:
particle: protons, 2.9 MeV
detector: 1 mm slotted CR-39 plate
method: Printed in the track-detector study, energy resolution section
status: ground
source: pmc-tasl-cr39
where: Energy resolution section, sentence on 2.9 MeV and 3.15 MeV protons
- benchmark: polymerization_time
label: Polymerization time, CR-39 comparative example
value: 18
unit: hours
scope: material
conditions:
temperature: not printed
initiator: not printed
method: Printed in a patent comparative example table
status: ground
source: patent-us5350822
where: Table 1, CR-39 column, polymerization time row
corrosion:
- environment: UV light (wavelength 254 nm and 365 nm, laboratory lamp)
headline: UV at 254 nm changes CR-39 optical absorption and its etch rate; UV at 365 nm did not change them in the cited study.
effect: At 254 nm the UV-Vis spectrum shows blue and red shifts and the band gap decreases with exposure time. At 365 nm there was no significant change in bulk etch rate or UV-Vis spectrum, even after 80 hours. The study also found that the bulk etch rate is modified by a factor that depends on the UV dose.
rating: moderate
conditions:
exposure: UV lamp 254 nm and 365 nm, 4 watt, samples 4 cm2
etchant: 6.25N NaOH at 70 °C
source: inoe-uv-padc
where: Abstract; Section 3.1 (effect of UV on the bulk etch rate)
- environment: Atomic oxygen in low Earth orbit (MISSE 2, ISS, 3.95 years)
headline: The erosion yield is above 6.80e-24 cm3/atom, so the sample eroded through before the end of the exposure.
effect: The lower-bound erosion yield exceeds the predicted value of 6.30e-24 cm3/atom, so the true yield is at least as high as the measured lower bound.
rating: severe
conditions:
exposure: MISSE 2 PEACE tray, ISS, outside the Quest airlock, 2001 to 2005
source: nasa-tm2008
where: Table I and Table VII
risks:
hazards:
- text: 'Diallyl diglycol carbonate, the liquid monomer (CAS 142-22-3): GHS hazard statements H302, H315 and H410 with signal word Warning, pictograms GHS07 and GHS09.'
ghs:
- H302
- H315
- H410
source: wikipedia-adc
where: Infobox, Hazards (GHS)
- text: No GHS classification for the cured polymer was read in this run. The hazard statements above describe the uncured monomer.
ghs: []
source: wikipedia-cr39
where: Infobox and lead section (no hazard data printed for the polymer)
failure_risks:
- mode: UV-induced change in optical absorption and etch behaviour
trigger: Exposure to short-wavelength UV (254 nm in the cited study)
consequence: Optical absorption rises and etch behaviour changes, so calibration of the track detector can drift. Changes at 365 nm were not measurable in the study.
severity: moderate
source: inoe-uv-padc
where: Abstract; Section 3.1
- mode: Atomic oxygen erosion in low Earth orbit
trigger: Long exposure to atomic oxygen on the ISS, MISSE 2 PEACE tray
consequence: The sample eroded through in the MISSE 2 flight, so its erosion yield is only a lower bound.
severity: critical
source: nasa-tm2008
where: Table I
handling:
- text: Keep continuous use at or below 100 °C, since the Wikipedia article gives 130 °C only for up to one hour and marks it as citation needed.
source: wikipedia-cr39
where: Applications, Optics section
- text: Handle the liquid monomer with the GHS precautions printed for it (H302, H315, H410); the cured polymer was not classified in the pages read.
source: wikipedia-adc
where: Infobox, Hazards (GHS)
uses:
- application: optics-and-cameras
device: Eyeglass and sunglass lenses
example: CR-39 lenses weigh about half as much as glass, and the first CR-39 lenses were made in 1947 by the Armorlite Lens Company.
source: wikipedia-cr39
where: Applications, Optics section, and History
- application: radiation-shielding
device: Solid-state nuclear track detector (dosimetry, not shielding)
example: CR-39 records tracks from alpha particles, neutrons, protons and radon, and is etched in concentrated sodium hydroxide to reveal them.
source: pmc-tasl-cr39
where: Introduction and Experimental set-up, sections 1 and 2
- application: structures
device: Space exposure test sample (MISSE 2, flight)
example: ADC (CR-39) flew on the MISSE 2 PEACE tray on the ISS from 2001 to 2005, and its erosion yield is recorded in Table I.
source: nasa-tm2008
where: Table I and Section 2.1 (exposure)
supply:
- subject: Diethylene glycol bis(allyl carbonate) monomer (ADC)
demand: Not read in this run. The monomer is used for cast optical lenses and track detectors (Wikipedia).
producers:
- name: PPG Industries
note: Named as trademark owner of CR-39 on the Wikipedia page (no volume or share read)
country: United States
critical_lists: []
substitutes: []
source: wikipedia-cr39
where: History and trademark sections
- subject: CR-39 track detectors (sold to researchers)
demand: Track Analysis Systems Ltd (UK) has served researchers in over 80 countries since 2013 (Wikipedia). No volume was read.
producers:
- name: Track Analysis Systems Ltd
note: Radiation track detector supplier, UK (Wikipedia, radiation detection section)
country: United Kingdom
- name: BlankSlate Innovation
note: Custom CR-39 and automated analysis services, US (Wikipedia)
country: United States
- name: Nagase Landauer
note: CR-39 for personal radiation dosimetry, Japan (Wikipedia)
country: Japan
critical_lists: []
substitutes: []
source: wikipedia-adc
where: Suppliers (radiation detection section)
documents:
- title: Atomic Oxygen Erosion Yield Predictive Tool for Spacecraft Polymers in Low Earth Orbit, NASA/TM-2008-215490
type: report
url: https://ntrs.nasa.gov/citations/20090011780
year: 2008
- title: US patent 5350822, High refractive index plastic lens composition (Comparative Example 2 for CR-39)
type: paper
url: https://patents.google.com/patent/US5350822
year: 1994
- title: US patent 6417273, Monomer composition for optical plastic material (Comparative Example 1, commercial ADC)
type: paper
url: https://patents.google.com/patent/US6417273B1/en
year: 2002
- title: Track Analysis Systems CR-39 detector study, PMC open-access article
type: paper
url: https://pmc.ncbi.nlm.nih.gov/articles/PMC5438376/
year: 2017
- title: UV-Vis spectroscopic and chemical etching studies of CR-39 (PADC) exposed to ultraviolet radiation, Optoelectronics and Advanced Materials
type: paper
url: https://oam-rc.inoe.ro/articles/uv-vis-spectroscopic-and-chemical-etching-studies-of-cr-39-padc-exposed-to-ultraviolet-radiation/fulltext
year: 2011
gaps:
- No glass transition temperature from differential scanning calorimetry was found for the cured polymer. The only Tg value is the heat-resistance figure from a patent table (91 °C), which the patent identifies as the temperature of maximum tan delta.
- No outgassing data (total mass loss, CVCM) for CR-39 was found in an opened source.
- No ECHA or PubChem classification was read for the cured polymer. PubChem returned a verification page, so the monomer hazard statements come from Wikipedia only.
- No current producer volumes or country shares for ADC or CR-39 were read. The supply section names suppliers and trademark owner only.
- No radiation dose or proton/electron damage value for CR-39 was read in an opened source.
- The cured polymer's repeat-unit formula was not printed in a fetched page; the formula given is the monomer's, C12H18O7.
- The NASA erosion yield for MISSE 2 is a lower bound (sample eroded through), so no full-flight yield is recorded.
- 'Non-canonical property names used: abbe_number, shrinkage (polymerization shrinkage, 13.6 %, is not in this file; see note), atomic_oxygen_erosion_yield, optical_absorption_coefficient, energy_resolution, polymerization_time, molar_mass, light_transmittance.'
- Polymerisation shrinkage of 13.6 % (patent Table 1) and the Abbe number 58 (patent Table 1, Wikipedia) were read but are not entered as properties because their names are not in the canonical list; they are in the patent source for reference.
- The Track Analysis Systems TASTRAK datasheet was not reached; its etch rates and thickness options are not recorded.
sources:
nasa-tm2008:
title: Atomic Oxygen Erosion Yield Predictive Tool for Spacecraft Polymers in Low Earth Orbit, NASA/TM-2008-215490 (Banks, Backus, de Groh)
url: https://ntrs.nasa.gov/citations/20090011780
kind: report
year: 2008
license: public domain (NASA)
wikipedia-cr39:
title: CR-39, Wikipedia (density, refractive index, Abbe number, heat limits, optics and detector use, history)
url: https://en.wikipedia.org/wiki/CR-39
kind: web
year: 2026
license: CC BY-SA 4.0
wikipedia-adc:
title: Diallyl diglycol carbonate (ADC monomer), Wikipedia (monomer properties, GHS hazards, suppliers)
url: https://en.wikipedia.org/wiki/Allyl_diglycol_carbonate
kind: web
year: 2026
license: CC BY-SA 4.0
wikipedia-ssntd:
title: Solid-state nuclear track detector, Wikipedia (CR-39 as a track detector)
url: https://en.wikipedia.org/wiki/Solid-state_nuclear_track_detector
kind: web
year: 2026
license: CC BY-SA 4.0
patent-us5350822:
title: US5350822, High refractive index plastic lens composition (Table 1 and Table 3, CR-39 comparative example)
url: https://patents.google.com/patent/US5350822
kind: paper
year: 1994
license: patent document (cited, not reproduced)
patent-us6417273:
title: US6417273, Monomer composition for optical plastic material (Table 4, commercial ADC plates)
url: https://patents.google.com/patent/US6417273B1/en
kind: paper
year: 2002
license: patent document (cited, not reproduced)
pmc-tasl-cr39:
title: CR-39 track detector for multi-MeV ion spectroscopy, PMC open-access article
url: https://pmc.ncbi.nlm.nih.gov/articles/PMC5438376/
kind: paper
year: 2017
license: open-access article (cited, not reproduced)
inoe-uv-padc:
title: UV-Vis spectroscopic and chemical etching studies of CR-39 (PADC) exposed to ultraviolet radiation, Optoelectronics and Advanced Materials
url: https://oam-rc.inoe.ro/articles/uv-vis-spectroscopic-and-chemical-etching-studies-of-cr-39-padc-exposed-to-ultraviolet-radiation/fulltext
kind: paper
year: 2011
license: open-access article (cited, not reproduced)
license: CC-BY-4.0
updated: '2026-10-20'
review:
status: draft
method: assistant
checked_values: 19
unreachable: 2
caveats: 4
note: 'Values read by an AI assistant on 2026-10-20 from the pages named in each entry. Unreachable: PubChem (reCAPTCHA page), ECHA (HTTP 403). The US patent 6417273 scanned PDF was image-only; its HTML page was read instead. The NASA erosion value is a lower bound.'
story:
recipe:
line: Poly(allyl diglycol carbonate) is made by polymerising the liquid monomer diethylene glycol bis(allyl carbonate), C12H18O7 (NASA Table IV; Wikipedia). The monomer is cured with a peroxide initiator, diisopropyl peroxydicarbonate, over about 18 hours (patent Table 1). The allyl groups crosslink, which makes the polymer a thermoset with no melting point.
parts:
- name: Diethylene glycol bis(allyl carbonate), allyl diglycol carbonate
symbol: ADC
role: Monomer. Its allyl groups crosslink on polymerisation.
share_note: Molar mass 274.2700 g/mol (NASA Table IV)
- name: Diisopropyl peroxydicarbonate
symbol: IPP
role: Initiator for the radical cure. Benzoyl peroxide is an alternative that gives a higher yellowness index (Wikipedia).
share_note: Share not read
risk_groups:
- title: For people
lead: The monomer carries H302, H315 and H410 hazard statements. The cured polymer was not classified in the pages read.
level: 1
verdict: Monomer hazardous, polymer not classified
points:
- label: Liquid monomer
line: Diallyl diglycol carbonate has GHS statements H302, H315 and H410 with signal word Warning (Wikipedia).
- title: If it fails
lead: UV and atomic oxygen both change the material, and the MISSE 2 sample eroded through.
points:
- label: UV at 254 nm
line: UV at 254 nm raises optical absorption to 54 cm-1 in the 215-242 nm band, while UV-A at 315-400 nm gives only 1 cm-1 (Section 2).
- label: Atomic oxygen in orbit
line: The MISSE 2 erosion yield is greater than 6.80e-24 cm3/atom after 3.95 years on the ISS, so the true yield is at least that.
- title: Handling and storage
points:
- label: Keep under the heat limit
line: Continuous use is up to 100 °C for optics (Wikipedia).
why: 'CR-39 is a clear, light plastic: its refractive index is 1.498, its specific gravity is 1.32 and it transmits 91 % of light in the patent comparison. Its heat resistance is 91 °C, and it weighs about half as much as glass. It is also a reliable track detector, with energy resolution of 3 % for 2.9 MeV protons.'
can_do:
- label: Let light through
value: 91 % light transmittance
benchmark: light_transmittance
line: The CR-39 comparative example in the patent transmits 91 % of light, and a commercial 2 mm ADC plate transmits 92 %.
- label: Bend light well
value: 1.498 refractive index
benchmark: refractive_index
line: The cured plastic has a refractive index of 1.498, close to the value for crown glass, per Wikipedia.
- label: Detect particles
value: 3 % energy resolution for 2.9 MeV protons
benchmark: energy_resolution
line: The track-detector study reports 3 % energy resolution for 2.9 MeV protons and 4 % for 3.15 MeV.
- label: Stay clear in heat
value: 100 °C continuous use
benchmark: max_service_temp
line: CR-39 is rated for continuous use up to 100 °C, and up to one hour at 130 °C per Wikipedia (citation needed).
uses:
- where: Eyeglass lenses
line: CR-39 lenses weigh about half as much as glass, and the first were made in 1947.
- where: Track detectors
line: CR-39 records alpha particles, neutrons, protons and radon, and is etched in sodium hydroxide to reveal tracks.
- where: Space test
line: ADC (CR-39) flew on the MISSE 2 PEACE tray on the ISS from 2001 to 2005, with an erosion yield greater than 6.80e-24 cm3/atom.
compare: The patent comparison puts CR-39 at 91 % light transmittance and a 1.498 refractive index. These are single comparative examples, so they are examples rather than a ranking against other optical plastics.
compare_rows:
- scope: material
label: Density
benchmark: density
- scope: material
label: Light transmittance
benchmark: light_transmittance
- scope: material
label: Atomic oxygen erosion yield
benchmark: atomic_oxygen_erosion_yield
handling:
- Keep continuous use at 100 °C or below. Expect UV to change optical absorption at 254 nm.
good_for:
- 'Light optical parts: 1.498 refractive index and 91 % light transmittance in the patent comparison.'
- 'Track detection: 3 % energy resolution for 2.9 MeV protons in the track-detector study.'
- 'Weight: about half the weight of glass for eyeglass lenses (Wikipedia).'
watch_out:
- 'Atomic oxygen: the MISSE 2 sample eroded through, with an erosion yield greater than 6.80e-24 cm3/atom.'
- 'UV at 254 nm: optical absorption reaches 54 cm-1 in the 215-242 nm band, and etch behaviour changes.'
- 'Monomer hazards: H302, H315 and H410 apply to the liquid monomer, and the cured polymer was not classified.'
verdict: CR-39 is a clear, light thermoset with 1.498 refractive index, 91 % light transmittance and 100 °C continuous use, which suits eyeglass lenses and track detection. It is weak in low Earth orbit, where the MISSE 2 sample eroded through, and under short-wavelength UV.
References