Aliphatic polyketone (PK, POKETONE, AKROTEK PK) PK

Copolymer of carbon monoxide with ethylene and a minor amount of propylene (aliphatic polyketone). PEVA is ethylene-vinyl acetate, 28 wt% vinyl acetate in the Vinmar EV0628 grade. · CAS 88995-51-1

Also known as POKETONE, M33AS1A-NP0, AKROTEK, Carilon, VINPOL EV0628

Aliphatic polyketone (PK) is a semi-crystalline thermoplastic made from carbon monoxide with ethylene and, in terpolymers, a little propylene.

12 sources · Updated 2026-10-26 · CC BY 4.0

Evidence level

2 of 5

Lab-measured

Melting range

> 220 °C

Melt flow

49 g/10 min

PEVA softening

49 °C

Recipe, share of the weight

  • CO not statedCarbon monoxide
  • not statedEthylene
  • not statedPropylene
  • not statedVinyl acetate

Best for

Injection-moulded and extruded ground parts that need wear resistance and resistance to hot water and weak chemicals (PK)

Weakest at

UV and heat ageing: no UV or heat-ageing number was read for PK, and the Akro-Plastic chemical table shows large yield-stress losses in hot acid and in dimethylformamide

Risk at a glance

  • People None found. Polymer not classed; monomers are hazardous
  • If it fails High. Strength loss in hot strong acid or solvent
  • Corrosion Severe. Hot concentrated sulphuric acid cuts yield stress by 72 % (table grade not named).

Quick facts: PK

Key properties of PK
PropertyValueBasis
Density0.95 g/cm³1 sourced value
Tensile strength19 MPa1 sourced value
Melting point75 to 248 °C5 sourced values across conditions

What is the density of Aliphatic polyketone (PK)?

Aliphatic polyketone (PK) has a density of 0.95 g/cm³. The source and test conditions are listed in the properties table on this page.

What is the melting point of Aliphatic polyketone (PK)?

Aliphatic polyketone (PK) has a melting point of 75 to 248 °C. The range covers 5 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What is the tensile strength of Aliphatic polyketone (PK)?

Aliphatic polyketone (PK) has a tensile strength of 19 MPa. The source and test conditions are listed in the properties table on this page.

What are the other names and codes for Aliphatic polyketone (PK)?

Aliphatic polyketone (PK) is also written as POKETONE, M33AS1A-NP0, AKROTEK, Carilon, VINPOL EV0628. Each code is printed in the source listed beside it in the designations table.

What is Aliphatic polyketone (PK) used for?

Uses recorded in the sources include Injection-moulded electrical, electronics, consumer and vehicle parts (ground); Wear-resistant, low-noise moving parts (ground); Ethylene-vinyl acetate encapsulant in photovoltaic modules (PEVA).

Why it exists

Polyketone is in this file as a thermoplastic that combines a melting range above 220 degC with documented resistance to hot water and weak chemicals, and as a plastic whose supplier SDS gives no hazard classification. PEVA is included briefly because it is the ethylene-vinyl acetate film used as a PV module encapsulant, and because its UV yellowing is documented in a 2017 study. Both polymers are ground-tested materials; no orbital or lunar test value was read for either.

Where it's used

Moulded electrical and vehicle parts

Hyosung names electrics and electronics, consumer goods, healthcare, mechanical engineering, vehicle construction and e-mobility as target segments for POKETONE.

Wear-resistant moving parts

The flyer says POKETONE has excellent wear resistance compared with other engineering polymers and reduces various noise problems. This is a ground use.

PV module encapsulant (PEVA)

The IIETA abstract says EVA is the most usually employed polymer for PV module encapsulant, because of its moderate cost and ease of implementation.

Recipe

Copolymer of carbon monoxide with ethylene and a minor amount of propylene (aliphatic polyketone). PEVA is ethylene-vinyl acetate, 28 wt% vinyl acetate in the Vinmar EV0628 grade.

Polyketone is a copolymer of carbon monoxide with olefins. The usual form is the ethylene-CO copolymer, and a small share of propylene gives a terpolymer with a slightly lower melting point (Wikipedia). The Akrotek page says roughly half of the chemical components come from carbon monoxide. PEVA is an ethylene and vinyl acetate copolymer, with 28 wt% vinyl acetate in the Vinmar EV0628 grade.

What PK is made of
IngredientShare of the weightWhat it does
Carbon monoxide CO not stated Adds the ketone groups along the chain. The ketone is what makes the polymer a polyketone.
Ethylene not stated Main olefin in the ethylene-CO copolymer. The PMC review calls it a cheap and plentiful monomer.
Propylene not stated Lowers the melting point a little in the terpolymer (Wikipedia).
Vinyl acetate not stated Comonomer in PEVA. Higher vinyl acetate content gives softer, more flexible grades (Wikipedia).

Weight shares are as printed in the sources.

What it can do

Melting range

> 220 °C

measured

The SDS gives a melting range above 220 degC for POKETONE M33AS1A, and the Akrotek page gives 220 degC for aliphatic polyketone in general.

Melt flow

49 g/10 min

measured

Melt flow index is 49 g/10 min for M33AS1A and 6 g/10 min for M630F, at 240 degC and 2.16 kg (flyer).

PEVA softening

49 °C

measured

The 28 wt% PEVA grade softens at 49 degC Vicat and peaks at 75 degC by DSC, so its use temperature is far below that of polyketone.

How it compares

Polyketone melts above 220 degC, while the 28 wt% PEVA grade softens at 49 degC Vicat and melts at 75 degC. Polyketone's water and chemical resistance comes from its maker and from one 2017 study, with no UV number. PEVA's UV yellowing comes from a 2017 PV paper, with no dose or duration. Neither polymer has an ageing number in this file.

The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.

Benchmarks
MeasurementPKCOCEPDMHDPEPMP (TPX)PEPPPVCUHMWPE
Thermal behavior and safety
Melting range, POKETONE M33AS1A (supplier SDS)> 220 °C1no datano data130 to 135 °C232 °C128 °C140 °Cno data135 °C
Melting point, aliphatic polyketone (product page)Statement on the Akro-Plastic Akrotek PK page220 °Cno datano data130 to 135 °C232 °C128 °C140 °Cno data135 °C
Melting range, non-alternating polyketones from Pd5 and Pd6 catalysts (lab)Range printed in the review text220 to 230 °Cno datano data130 to 135 °C232 °C128 °C140 °Cno data135 °C
Melting point across CO/ethylene feed ratios 1/1 to 1/20 (lab)147 to 248 °C2no datano data130 to 135 °C232 °C128 °C140 °Cno data135 °C
Peak melting point by DSC, PEVA 28 wt% VA (Vinmar EV0628)ASTM D-3418 peak melting point by DSC as printed75 °Cno datano data130 to 135 °C232 °C128 °C140 °Cno data135 °C
Physical and electrical
Density, PEVA 28 wt% VA (Vinmar EV0628)ASTM D-1505 as printed0.948 g/cm³1020 kg/m31.19 g/cm³0.959 g/cm³833 kg/m30.959 g/cm³0.9 g/cm³1.32 g/cc0.93 g/cc
Durometer hardness, PEVA grade EV0628ASTM D-2240 as printed85 Shore Ano datano datano datano datano datano datano datano data
Temperature behavior
Autoignition temperature, POKETONE M33AS1APrinted in the supplier SDS> 250 °Cno datano datano datano datano datano datano datano data
Vicat softening temperature, PEVA 28 wt% VA (Vinmar EV0628)ASTM D-1525 as printed49 °C133 °Cno data80 °C168 °Cno data130 °C79 to 81 °Cno data
Other measurements
Flash point, POKETONE M33AS1A> 93 °C3no datano datano datano datano datano datano data> 662 °F
Burning rate, POKETONE M33AS1A (UN test N1)< 0.7 mm/s4no datano datano datano datano datano datano datano data
Melt flow index, POKETONE M33AS1A (modified, silicone)49 g/10 min5no datano data18 g/10 min26 g/10minno data12 g/10 minno datano data
Melt flow index, POKETONE M630F (unreinforced extrusion grade)6 g/10 min6no datano data18 g/10 min26 g/10minno data12 g/10 minno datano data
Elongation at yield, AKROTEK PK (general)Printed on the Akro-Plastic product page25 %120 %255 %> 400 %22 %400 %no data140 %300 %
Tensile strength at break, PEVA 28 wt% VA (Type IV)ASTM D-638 as printed19 MPa746 MPa10.5 MPano data25 MPa21 MPano data33 MPa40 MPa
Elongation at break, PEVA 28 wt% VA (Type IV)ASTM D-638 as printed1100 %120 %255 %> 400 %22 %400 %no data140 %300 %
1 % secant flexural modulus, PEVA 28 wt% VAASTM D-790 as printed24 MPano datano data13000 kg/cm²1450 MPano data1480 MPa2.65 GPa0.6 GPa
Melt index, PEVA 28 wt% VA (Vinmar EV0628)ASTM D-1238 as printed6 g/10 minno datano data18 g/10 min26 g/10minno data12 g/10 minno datano data
Vinyl acetate content, PEVA grade EV062828 wt%8no datano datano datano datano datano datano datano data

Why choose it, and why not

Good for

  • Wear-resistant, low-noise moulded parts, as the flyer describes.
  • Parts exposed to hot water or weak acids and alkalis, where the maker and a 2017 study report little loss.
  • PEVA as a PV module encapsulant film, the role the IIETA abstract describes.

Watch out for

  • UV: no PK UV test result was read. PEVA yellows and loses adhesion under extended UV.
  • Hot acids and solvents: 40 % sulphuric acid and dimethylformamide at 80 degC cut yield stress by 72 % and 80 % in the table, and DMF swells and dissolves the samples.
  • A melting point of 220 degC is not a service temperature. No heat-ageing data were read.
  • The density of polyketone is not recorded, because the SDS prints it with no unit.

Polyketone is a lightly documented engineering thermoplastic. Its SDS shows no GHS hazard, its melting range is above 220 degC, and its water and chemical resistance is supported by a maker flyer, a supplier table and one study. Its UV and heat ageing are not measured here. PEVA is covered only briefly, with datasheet values but no ageing numbers.

Technical details

For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.

Other names and standards

The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.

Other names and standards
SystemCodes
Trade namePOKETONE, M33AS1A-NP0, AKROTEK, Carilon, VINPOL EV0628

Notes

The method, full conditions and any caveat for the numbered rows above.

Notes for the numbered rows
#MeasurementMethodConditionsCaveat
1Melting range, POKETONE M33AS1A (supplier SDS)Melting range as printed in the supplier safety data sheetgrade POKETONE M33AS1A-NP0 pellet, as printed in the SDSnote on bound printed as a range greater than 220 °C—
2Melting point across CO/ethylene feed ratios 1/1 to 1/20 (lab)Range printed in the review text, decreasing from 248 degC to 147 degCbasis laboratory polyketones from a Pd38 catalyst; melting temperature falls as the ethylene feed risesfeed ratio CO/ethylene 1/1 to 1/20—
3Flash point, POKETONE M33AS1APrinted in the supplier SDS, rapid equilibrium methodmethod note rapid equilibrium method, as printedprinted as no flash occurred under 93 °C—
4Burning rate, POKETONE M33AS1A (UN test N1)Printed in the supplier SDS, flammability sectiontest UN TDG test and criteria, test N1, as printed—
5Melt flow index, POKETONE M33AS1A (modified, silicone)Melt-flow index column of the POKETONE portfolio tabletemperature load 240 °C / 2.16 kg as printed in the flyer headerstandard ASTM D1238, ISO 1133 as printed—
6Melt flow index, POKETONE M630F (unreinforced extrusion grade)Melt-flow index column of the POKETONE portfolio tabletemperature load 240 °C / 2.16 kg as printed in the flyer headerstandard ASTM D1238, ISO 1133 as printed—
7Tensile strength at break, PEVA 28 wt% VA (Type IV)—grade VINPOL EV0628, 28 wt% vinyl acetateprinted as 2,800 (19) psi (MPa)specimen Type IV—
8Vinyl acetate content, PEVA grade EV0628Printed in the resin property table, Vinyl Acetate Contentmethod note supplier method, as printed—

Corrosion and compatibility

What happens when it meets other materials and environments.

Corrosion and compatibility
EnvironmentConcernWhat happens
Hot 40 % sulphuric acid (80 degC, 3 months) severe Hot concentrated sulphuric acid cuts yield stress by 72 % (table grade not named).1
Dimethylformamide at 80 degC (6 months) severe Dimethylformamide swells PK and slowly dissolves it at 80 degC.2
Humid air and hot glycol-water (moisture uptake) low Polyketone barely absorbs water and keeps its strength in hot glycol-water.3
Hot glycol-water, glass-fibre polyketone composites at 120 degC low Glass-fibre PK held its mechanical properties in 120 degC glycol-water better than PA 66.4
UV exposure of PEVA encapsulant in PV modules moderate Extended UV exposure makes EVA yellow and lose adhesion.5
UV exposure of POKETONE (UV-stabilised and standard grades) not rated No UV test result was read for PK.6
Heat above the Vicat point (PEVA) and the melting range (PK) not rated No heat-ageing data read; the datasheet values are softening and melting points, not ageing limits.7
Corrosion details
#EnvironmentDetailsTest conditions
1 Hot 40 % sulphuric acid (80 degC, 3 months) The Akro-Plastic PK resistance table reports a change in yield stress of -72 % after 3 months at 80 degC in sulphuric acid 40 %, with the surface turned black. At 23 degC for 12 months the same acid gave no change in yield stress. basis table of subjective classifications following ISO 175 and related standards; the grade is not named in the table
2 Dimethylformamide at 80 degC (6 months) The table reports a yield-stress change of -80 % after 6 months at 80 degC in dimethylformamide, with samples swelling and slowly dissolving. At 23 degC for 12 months the change was -10 %. basis same resistance table; grade not named
3 Humid air and hot glycol-water (moisture uptake) Hyosung says POKETONE is hydrolysis resistant and hardly absorbs water. A 2017 study of glass-fibre polyketone composites in monoethylene glycol and water at 120 degC found no change or only slight drops in tensile strength, modulus and strain at break. The Akro-Plastic page reports only a minimal strength loss in hydrolysis testing against a polyamide comparison grade. No water-absorption number was read. basis maker statement, 2017 composite study (abstract), and supplier comparison; no moisture-uptake value was read
4 Hot glycol-water, glass-fibre polyketone composites at 120 degC The abstract says that increasing immersion time in the monoethylene glycol and water solution at 120 degC had no impact or slightly decreased tensile strength, tensile modulus and strain at break for POK composites, while PA 66 composites showed a significant drop. The abstract gives no numbers. basis composites with 30 to 50 % glass fibre, immersion times not given in the abstract
5 UV exposure of PEVA encapsulant in PV modules The IIETA abstract says that an extended exposure to UV causes a loss of adhesion and a reduction of optical transmission (yellowing) in EVA encapsulant. Newer EVA formulations with antioxidants and UV absorbers were developed, but the abstract says optical degradation is still the main cause of performance loss in a module. basis qualitative abstract statement for a standard EVA formulation in a glass/EVA/glass stack; no UV dose, duration or transmission value was read
6 UV exposure of POKETONE (UV-stabilised and standard grades) The Hyosung flyer lists UV-stabilised grades (M630F-UV and M63VX0A) but gives no UV or weathering result. The Akro-Plastic PK pages list no UV data. The UV rating is therefore unknown, not low. basis no UV test result read; grade labels only
7 Heat above the Vicat point (PEVA) and the melting range (PK) PEVA softens at 49 degC Vicat and peaks at 75 degC by DSC for the Vinmar grade. Polyketone melts above 220 degC and gives no autoignition below 250 degC. None of these is an oven-ageing time or temperature series, so the heat-ageing rating is unknown. basis softening and melting points only; no time at temperature was read

Risks and side effects

Hazards to people, what happens when a cell overheats, and how the material is handled and stored.

For people

The polyketone pellet is not classed under GHS by its supplier. PubChem classes the raw monomers, which are gases and liquids, not the solid polymer.

The pellet
The supplier SDS gives GHS as not applicable for physical, health and environmental hazards, with NFPA ratings 0 for health, 1 for flammability and 0 for reactivity.
Dust
The SDS asks users to avoid dust formation and to pick up spilled pellets without creating dust.
Monomers
PubChem lists carbon monoxide (H220, H280, H331, H360, H372) and vinyl acetate (H225, H332, H341, H351) as hazardous.

If the pellet burns

The SDS gives a burning rate below 0.7 mm/s (UN test N1) and no spontaneous combustion below 250 degC.

Flash
No flash occurred below 93 degC by the rapid equilibrium method.
Products
The SDS names carbon oxides as the hazardous decomposition products and advises self-contained breathing apparatus for fire fighters.

UV and heat in use

Heat and UV limits here come from datasheet softening and melting points and from qualitative literature. No ageing test value was read for either polymer.

PEVA softening
The Vinmar EV0628 sheet gives a Vicat softening point of 49 degC and a DSC peak melting point of 75 degC, which are test values, not service ratings.
EVA under UV
An extended UV exposure caused a loss of adhesion and a reduction in optical transmission (yellowing) in an EVA encapsulant, according to the IIETA abstract.

Test details
The original wording and numbers from the sources, for readers who want them.

Failure risks

Failure risks
FailureTrigger and consequence
Strength loss in hot strong acid or solventhigh severityImmersion at 80 degC, for example 40 % sulphuric acid for 3 months or dimethylformamide for 6 monthsYield stress changes of -72 % (sulphuric acid, 40 %) and -80 % (dimethylformamide), with samples swelling and dissolving in DMF. The grade is not named in the table.
UV degradation of polyketonemoderate severitySunlight or UV exposure in serviceNo UV test result was read for PK, so the effect size is unknown. UV-stabilised grades are sold, which suggests the base grade is not the choice for long UV exposure.
Yellowing and loss of adhesion in PEVA encapsulantmoderate severityExtended UV exposure of a glass/EVA/glass stackLoss of adhesion and a reduction in optical transmission. The abstract gives no dose, duration or percentage.
Softening of PEVAmoderate severityUse above the Vicat softening point (49 degC) or near the DSC peak melting point (75 degC)The datasheet values mark where the Vinmar EV0628 grade softens and melts. They are test values, not a service rating.
Burning of the pelletlow severityIgnition of pellets or dustBurning rate below 0.7 mm/s (UN test N1). The SDS gives no spontaneous combustion below 250 degC and no flash below 93 degC.

Side effects on surrounding parts

Side effects on surrounding parts
AffectsEffect
Fire fighters and people in the enclosureCombustion gives carbon oxides, which the SDS lists as hazardous decomposition products. No other decomposition product is given, and the SDS says no data are available for specific fire hazards.

Handling and storage

  • Avoid dust formation. Pick up spilled pellets without creating dust, and remove sources of ignition.
  • Keep away from strong oxidising agents, which the SDS lists as materials to avoid.

Mitigations

  • UV-stabilised grades are listed (M630F-UV and M63VX0A). The flyer gives no UV test result, so test the chosen grade before outdoor use.
  • Newer EVA formulations contain antioxidants and UV absorbers. The IIETA abstract says these were developed but gives no effect size.

Supply and geography

How common the raw materials are and where they come from.

Aliphatic polyketone resin (POKETONE, AKROTEK PK)

Ethylene (main olefin feedstock)