Ti-13V-11Cr-3Al (B120VCA beta titanium) Ti-13-11-3
Beta titanium alloy Ti-13V-11Cr-3Al, titanium balance with nominal 13 % vanadium, 11 % chromium and 3 % aluminium by weight
Also known as AMS 4917, MIL MIL-T-9046, MIL MIL-T-9046J, B120VCA, Ti-13-11-3
Ti-13V-11Cr-3Al is an age-hardening beta titanium alloy, specified to AMS 4917 for sheet, strip and plate and to MIL-T-9046J.
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Tensile strength (specification minimum)
861 MPa minimum
Yield strength (specification minimum)
827 MPa minimum
Powder density
4.58 g/cm3
Melting range (powder)
1630 to 1660 °C
Ageing temperature
482 °C
Recipe, share of the weight
- Ti balance (Bal.) as printedTitanium
- V 12.5 to 14.5%Vanadium
- Cr 10 to 12%Chromium
- Al 2.5 to 3.5%Aluminium
- Fe printed as 0.35, no rangeIron
- C maximum, printed as ≤0.05Carbon
- N maximum, printed as ≤0.08Nitrogen
- H maximum 250 ppm, as printedHydrogen
Best for
High-strength beta titanium sheet, strip and plate where AMS 4917 or MIL-T-9046J is specified
Weakest at
Wrought density, aged-condition strength and alloy-specific hazard data were not found in the sources held; the supplier powder figures disagree with the MIL minimums
Risk at a glance
- People No data. No hazard data recorded
- If it fails No data. No failure risks recorded
- Corrosion Low. The powder supplier says the alloy has good corrosion resistance, including in seawater.
Quick facts: Ti-13-11-3
| Property | Value | Basis |
|---|---|---|
| Density | 4.58 g/cm³ | 1 sourced value |
| Yield strength | 827 to 850 MPa | 2 sourced values across conditions |
| Tensile strength | 861 to 950 MPa | 2 sourced values across conditions |
| Young's modulus | 80 to 130 GPa | 2 sourced values across conditions |
| Thermal conductivity | 6.7 W/(m·K) | 2 sourced values across conditions |
| Melting point | 1,630 to 1,660 °C | 1 sourced value |
| Specific heat | 515 J/(kg·K) | 1 sourced value |
What is the density of Ti-13V-11Cr-3Al (Ti-13-11-3)?
Ti-13V-11Cr-3Al (Ti-13-11-3) has a density of 4.58 g/cm³. The source and test conditions are listed in the properties table on this page.
What is the thermal conductivity of Ti-13V-11Cr-3Al (Ti-13-11-3)?
Ti-13V-11Cr-3Al (Ti-13-11-3) has a thermal conductivity of 6.7 W/(m·K). The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the melting point of Ti-13V-11Cr-3Al (Ti-13-11-3)?
Ti-13V-11Cr-3Al (Ti-13-11-3) has a melting point of 1,630 to 1,660 °C. The source and test conditions are listed in the properties table on this page.
What is the yield strength of Ti-13V-11Cr-3Al (Ti-13-11-3)?
Ti-13V-11Cr-3Al (Ti-13-11-3) has a yield strength of 827 to 850 MPa. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the tensile strength of Ti-13V-11Cr-3Al (Ti-13-11-3)?
Ti-13V-11Cr-3Al (Ti-13-11-3) has a tensile strength of 861 to 950 MPa. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What are the other names and codes for Ti-13V-11Cr-3Al (Ti-13-11-3)?
Ti-13V-11Cr-3Al (Ti-13-11-3) is also written as AMS 4917, MIL MIL-T-9046, MIL MIL-T-9046J, B120VCA, Ti-13-11-3. Each code is printed in the source listed beside it in the designations table.
What is Ti-13V-11Cr-3Al (Ti-13-11-3) used for?
Uses recorded in the sources include Sheet, strip and plate in the solution-treated condition; Aircraft components and structural parts; Spherical powder feedstock for additive manufacturing (3D printing).
Why it exists
Ti-13V-11Cr-3Al is a beta titanium alloy with high strength for its weight. The MIL-T-9046J minimums are 861 MPa tensile and 827 MPa yield at 0 - 30°C, with at least 3 % elongation, and AMS 4917 covers the alloy as sheet, strip and plate in the solution-treated condition. A supplier of the alloy powder reports 950 MPa tensile and 850 MPa yield, a higher figure with no temper or test temperature stated, so the two sets of values are shown side by side rather than merged.
Where it's used
Aircraft sheet, strip and plate
AMS 4917 covers this titanium alloy as sheet, strip and plate in the solution-treated condition, according to the SAE listing for AMS4917E.
Aircraft components and structural parts
The powder supplier says the alloy is widely used in aerospace applications, such as aircraft components or structural parts.
Additive manufacturing feedstock
The same supplier offered the alloy as spherical powder for making complex components by additive manufacturing. The catalog entry is now discontinued.
Recipe
Beta titanium alloy Ti-13V-11Cr-3Al, titanium balance with nominal 13 % vanadium, 11 % chromium and 3 % aluminium by weight
Ti-13V-11Cr-3Al is a titanium alloy: titanium is the balance, and vanadium, chromium and aluminium are the alloying additions. Supplier and specification pages print composition limits as percent by weight. The SAE page gives the heat treatment that follows melting and forming, a solution treatment and then ageing.
| Ingredient | Share of the weight | What it does |
|---|---|---|
| Titanium Ti | balance (Bal.) as printed | Base metal, the balance of the alloy |
| Vanadium V | 12.5 to 14.5% | Main alloying element |
| Chromium Cr | 10 to 12% | Alloying element |
| Aluminium Al | 2.5 to 3.5% | Alloying element |
| Iron Fe | printed as 0.35, no range | Impurity, as printed |
| Carbon C | maximum, printed as ≤0.05 | Impurity limit |
| Nitrogen N | maximum, printed as ≤0.08 | Impurity limit |
| Hydrogen H | maximum 250 ppm, as printed | Impurity limit |
Weight shares are as printed in the sources.
What it can do
Tensile strength (specification minimum)
861 MPa minimum
measured
Under MIL-T-9046J the tensile strength is at least 861 MPa at 0 - 30°C, per the Total Materia MIL table.
Yield strength (specification minimum)
827 MPa minimum
measured
The Rp0.2 yield strength is at least 827 MPa in the same table, with at least 3 % elongation.
Powder density
4.58 g/cm3
measured
The spherical powder has a density of 4.58 g/cm3 as printed by the supplier. A wrought density was not found.
Melting range (powder)
1630 to 1660 °C
measured
The supplier powder prints a melting range of 1630 to 1660 °C.
Ageing temperature
482 °C
measured
After solution treatment at 788 to 816 °C, the SAE page gives ageing at 482 °C for 2 to 60 hours.
Elastic modulus
80 to 130 GPa
measured
The modulus is printed as 80 to 130 GPa on the MIL and SAE Total Materia pages. The test temperature is not clear in the extracted row.
How it compares
The MIL-T-9046J minimums (861 MPa tensile and 827 MPa yield) are lower than the powder supplier's stated values (950 MPa tensile and 850 MPa yield). A minimum is a floor a specification guarantees, while the supplier figure is a single product value with no temper or test temperature, so the two should not be ranked against each other. The thermal conductivity also differs by source: 8.044 W/(m∙°C) on the MIL page against 6.7 W/(m*K) for the powder.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | Ti-13-11-3 | CP Ti Grade 2 | Ti-6Al-4V | Ti-6Al-4V ELI | Ti-3Al-2.5V (Grade 9) | TiAl | Beta 3 | Ti Grade 11 | Ti Gr 12 | CP Ti Grade 3 | CP Ti Grade 7 | Ti minor alloys |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Thermal behavior and safety | ||||||||||||
| Melting range, spherical powder of Ti-13V-11Cr-3AlRange printed on a supplier product page | 1630 to 1660 °C2 | no data | 1604 °C | 1650 to 1660 °C | no data | no data | 3000 degF | 1670 °C | 1660 °C | no data | no data | 3000 degF |
| Thermal conductivity, MIL Ti-13V-11Cr-3Al | 8.044 W/(m∙°C)7 | 22 W/(m·K) | 6.7 W/(m K) | 6.6 W/(m K) | no data | no data | no data | 21.79 W/(m·K) | 19.02 W/(m·K) | 151.2 Btu-in/(hr·ft²·°F) | 21.79 W/m-K | 46.8 BTU-in/hr-ft2-°F |
| Thermal conductivity, spherical powderValue printed on a supplier product page | 6.7 W/(m*K)12 | 22 W/(m·K) | 6.7 W/(m K) | 6.6 W/(m K) | no data | no data | no data | 21.79 W/(m·K) | 19.02 W/(m·K) | 151.2 Btu-in/(hr·ft²·°F) | 21.79 W/m-K | 46.8 BTU-in/hr-ft2-°F |
| Specific heat capacity, spherical powderValue printed on a supplier product page | 515 J/(kg*K)13 | no data | 0.526 J/(g K) | 0.58 J/(g K) | no data | no data | no data | no data | 544 J/(kg·K) | no data | no data | no data |
| Physical and electrical | ||||||||||||
| Density, spherical powder of Ti-13V-11Cr-3AlValue printed on a supplier product page | 4.58 g/cm³1 | 4.51 g/cm³ | 4.43 g/cm³ | 4.42 g/cm³ | 4.48 g/cm³ | 3.8 g/cm³ | 5.07 g/cm³ | 4.51 g/cm³ | 4.51 g/cm³ | 4.51 g/cm³ | 4.51 g/cm³ | 4.54 g/cm³ |
| Temperature behavior | ||||||||||||
| Solution treatment temperature, SAE heat treatment | 788 to 816 °C21 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Ageing temperature, SAE heat treatment | 482 °C22 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Other measurements | ||||||||||||
| Tensile strength Rm, MIL-T-9046J minimum | > 861 MPa3 | > 345 MPa | no data | 828 MPa | > 620 MPa | 422 MPa | 1000 MPa | > 240 MPa | > 483 MPa | > 450 MPa | > 345 MPa | < 175 ksi |
| Yield strength Rp0.2, MIL-T-9046J minimum | > 827 MPa4 | > 275 MPa | 830 MPa | 759 MPa | > 483 MPa | 326 MPa | 965 MPa | > 138 MPa | > 345 MPa | > 380 MPa | > 275 MPa | < 186 ksi |
| Elongation A, MIL-T-9046J minimum | > 3 %5 | > 20 % | 10 % | 10 % | > 15 % | 1.7 % | 7 % | > 24 % | > 18 % | > 18 % | > 20 % | < 10 % |
| Modulus of elasticity, MIL Ti-13V-11Cr-3Al | 80 to 130 GPa6 | 103 GPa | 113.8 GPa | 107 to 122 GPa | 91 GPa | 168 GPa | 82 GPa | 112 GPa | 103 GPa | 103 GPa | 112 GPa | 15000 ksi |
| Tensile strength (ultimate), spherical powderValue printed on a supplier product page | 950 MPa8 | > 345 MPa | no data | 828 MPa | > 620 MPa | 422 MPa | 1000 MPa | > 240 MPa | > 483 MPa | > 450 MPa | > 345 MPa | < 175 ksi |
| Yield strength, spherical powderValue printed on a supplier product page | 850 MPa9 | > 275 MPa | 830 MPa | 759 MPa | > 483 MPa | 326 MPa | 965 MPa | > 138 MPa | > 345 MPa | > 380 MPa | > 275 MPa | < 186 ksi |
| Elongation at break, spherical powderValue printed on a supplier product page | 7 %10 | > 20 % | 10 % | 10 % | > 15 % | 1.7 % | 7 % | > 24 % | > 18 % | > 18 % | > 20 % | < 10 % |
| Elastic modulus, spherical powderValue printed on a supplier product page | 103 GPa11 | 103 GPa | 113.8 GPa | 107 to 122 GPa | 91 GPa | 168 GPa | 82 GPa | 112 GPa | 103 GPa | 103 GPa | 112 GPa | 15000 ksi |
| Vanadium content, supplier powder specification | 12.5 to 14.5 %14 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Chromium content, supplier powder specification | 10 to 12 %15 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Aluminium content, supplier powder specification | 2.5 to 3.5 %16 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Iron content, supplier powder specification | < 0.35 %17 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Carbon content, supplier powder specification | < 0.05 %18 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Nitrogen content, supplier powder specification | < 0.08 %19 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Hydrogen content, supplier powder specification | < 250 ppm20 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Ageing time, SAE heat treatment | 2 to 60 hours23 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
Why choose it, and why not
Good for
- Sheet, strip and plate for aircraft structures, where MIL-T-9046J sets minimum tensile and yield strengths.
- Age hardening after solution treatment, using the SAE heat treatment steps.
Watch out for
- The strength minimums carry no stated temper, so no aged-condition strength is recorded for sheet.
- The supplier powder and the MIL minimums disagree. Both are shown and neither is averaged.
- The wrought density and melting point were not found, so mass and melting data are powder values only.
- No hazard or failure data were found for this alloy.
Ti-13V-11Cr-3Al is a high-strength beta titanium alloy with MIL-T-9046J minimums of 861 MPa tensile and 827 MPa yield, and a published heat treatment of 788 to 816 °C solution treatment and 482 °C ageing. Its wrought density, aged-condition strength and alloy-specific hazard data are not in the sources held, and the supplier powder values differ from the specification minimums.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Other names and standards
The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.
| System | Codes |
|---|---|
| AMS | 4917 (sheet, strip and plate, solution heat treated) |
| MIL | MIL-T-9046 (titanium sheet, strip and plate), MIL-T-9046J |
| Trade name | B120VCA, Ti-13-11-3 (other name printed on the supplier page) |
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Density, spherical powder of Ti-13V-11Cr-3Al | — | form spherical powder, supplier catalog DP4828 (listed as discontinued)temperature not statedunit in source 4.58g/cm 3 | Powder value, not a wrought sheet value. The Total Materia MIL page shows a placeholder for wrought density. |
| 2 | Melting range, spherical powder of Ti-13V-11Cr-3Al | — | form spherical powderpressure not statedunit in source 1630~1660℃ | — |
| 3 | Tensile strength Rm, MIL-T-9046J minimum | Minimum value printed in a Total Materia table for the MIL specification | specification MIL-T-9046J: 1991temperature 0 - 30°C (column header as printed)temper not stated on the pageunit in source ≥ 861 MPa | A minimum for the specification, not a typical value. The same page prints 950 MPa for the supplier powder. |
| 4 | Yield strength Rp0.2, MIL-T-9046J minimum | Minimum value printed in a Total Materia table for the MIL specification | specification MIL-T-9046J: 1991temperature 0 - 30°C (column header as printed)temper not stated on the pageunit in source ≥ 827 MPa | — |
| 5 | Elongation A, MIL-T-9046J minimum | Minimum value printed in a Total Materia table for the MIL specification | specification MIL-T-9046J: 1991temperature 0 - 30°C (column header as printed)unit in source ≥ 3 % | — |
| 6 | Modulus of elasticity, MIL Ti-13V-11Cr-3Al | Range printed in a Total Materia physical properties table | specification MIL-T-9046J: 1991temperature not clearly stated in the extracted rowunit in source 80 — 130 GPa | The same 80 to 130 GPa range is printed on the SAE page (totalmateria-sae). |
| 7 | Thermal conductivity, MIL Ti-13V-11Cr-3Al | Value printed in a Total Materia physical properties table | specification MIL-T-9046J: 1991temperature not statedunit in source 8.044 W/(m∙°C) | Disagrees with 6.7 W/(m*K) on the supplier powder page; both are kept side by side. |
| 8 | Tensile strength (ultimate), spherical powder | — | form spherical powdertemperature not statedtemper not stated | Disagrees with the MIL minimum of 861 MPa; a supplier powder value with no temper or test temperature, not a specification minimum. |
| 9 | Yield strength, spherical powder | — | form spherical powdertemperature not statedtemper not stated | Disagrees with the MIL minimum of 827 MPa; a supplier powder value. |
| 10 | Elongation at break, spherical powder | — | form spherical powdertemperature not statedtemper not stated | — |
| 11 | Elastic modulus, spherical powder | — | form spherical powdertemperature not stated | Falls inside the MIL range of 80 to 130 GPa; shown as a supplier value next to that range. |
| 12 | Thermal conductivity, spherical powder | — | form spherical powdertemperature not statedunit in source 6.7W/(m*K) | Disagrees with 8.044 W/(m∙°C) on the MIL page. |
| 13 | Specific heat capacity, spherical powder | — | form spherical powdertemperature not statedunit in source 515 J/(kg*K) | — |
| 14 | Vanadium content, supplier powder specification | Range printed in the composition table of a supplier product page | form spherical powderbasis content as printed in the composition tableunit in source Content (%) | The MIL page prints a placeholder for vanadium; this row is the only printed vanadium range read. |
| 15 | Chromium content, supplier powder specification | Range printed in the composition table of a supplier product page | form spherical powderbasis content as printed in the composition tableunit in source 10.0~12.0 | — |
| 16 | Aluminium content, supplier powder specification | Range printed in the composition table of a supplier product page | form spherical powderbasis content as printed in the composition tableunit in source 2.5~3.5 | — |
| 17 | Iron content, supplier powder specification | Value printed in the composition table of a supplier product page | form spherical powderbasis single value printed, no rangeunit in source 0.35 | The table prints one value without a range or a label of maximum; it is shown as printed. |
| 18 | Carbon content, supplier powder specification | Limit printed in the composition table of a supplier product page | form spherical powderbasis maximum, printed as less than or equal tounit in source ≤0.05 | — |
| 19 | Nitrogen content, supplier powder specification | Limit printed in the composition table of a supplier product page | form spherical powderbasis maximum, printed as less than or equal tounit in source ≤0.08 | — |
| 20 | Hydrogen content, supplier powder specification | Limit printed in the composition table of a supplier product page | form spherical powderbasis maximumunit in source 250ppm. Max. | — |
| 21 | Solution treatment temperature, SAE heat treatment | Range printed in a Total Materia heat treatment section | hold within ±14°C (±25°F), then water quenched; sections may be air cooledunit in source 788 to 816°C (1450 to 1500°F) | Process parameter with no canonical benchmark name; recorded under solution_treatment_temperature. |
| 22 | Ageing temperature, SAE heat treatment | Value printed in a Total Materia heat treatment section | tolerance ±8°C (900°F ± 15°F)hold 2 to 60 hours, then air cooledunit in source 482°C ± 8°C (900°F ± 15°F) | Process parameter with no canonical benchmark name; recorded under aging_temperature. |
| 23 | Ageing time, SAE heat treatment | Range printed in a Total Materia heat treatment section | temperature 482°C ± 8°Cunit in source 2 to 60 hour | Process parameter with no canonical benchmark name; recorded under aging_time. |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Seawater and general corrosion, supplier statement | low | The powder supplier says the alloy has good corrosion resistance, including in seawater.1 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Seawater and general corrosion, supplier statement | Stanford Advanced Materials states that Ti-13-11-3 shows good corrosion resistance in the seawater environment, which suits marine use. The page gives no corrosion rate, test medium or exposure time. | basis supplier wording only; no test data printed on the page |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
No safety data sheet for this alloy or its powder was found in the sources held. The only GHS data read is for the element titanium.
- Powder
- The supplier product page prints no hazard classification, and no safety data sheet for the alloy was found.
If it fails
The sources give specification minimums and supplier values, not failure records.
- Strength floor
- The MIL-T-9046J minimums are 861 MPa tensile and 827 MPa yield at 0 - 30°C. The supplier powder values of 950 MPa and 850 MPa carry no temper or test temperature.
Handling and storage
- Heat treatment
- Solution treatment at 788 to 816 °C is followed by a water quench, and ageing at 482 °C for 2 to 60 hours, per the SAE page.
Test details
The original wording and numbers from the sources, for readers who want them.
Handling and storage
- Heat treat in two steps: solution treat at 788 to 816 °C and water quench, then age at 482 °C for 2 to 60 hours and air cool (SAE page).
- Lighter sections may be air cooled after solution treatment instead of water quenched (SAE page).
- Check the governing specification, AMS 4917 or MIL-T-9046J, before use. The full texts of both were not read.
Supply and geography
How common the raw materials are and where they come from.
Titanium sponge metal (feedstock for titanium alloys)
USGS reports world sponge metal production of 370,000 tons in 2025 (estimated), after 380,000 tons in 2024. Sponge is the metal feedstock for alloys such as this one.
- Top producers (2025)
- China, Japan, Russia, Kazakhstan, Saudi Arabia
- Recycling
- USGS: owing to limited responses from voluntary surveys, consumption data for titanium scrap metal for the titanium metal industry were withheld. The United States imported an estimated 44,000 tons of sponge in 2025 (estimated).
- Substitutes
- USGS: Aluminum, nickel, specialty steels, and zirconium alloys may be substituted for titanium for applications that require corrosion resistance.; USGS: In high-strength applications, titanium competes with aluminum, composites, intermetallics, steel, and superalloys.
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: titanium-13v-11cr-3al
spore_version: 0.2
family: titanium-alloys
name: Ti-13V-11Cr-3Al (B120VCA beta titanium)
abbreviation: Ti-13-11-3
role: Age-hardening beta titanium alloy for sheet, strip and plate
category: metals
type: titanium
summary: |
Ti-13V-11Cr-3Al is an age-hardening beta titanium alloy, specified to AMS 4917 for sheet, strip and plate and to MIL-T-9046J. The MIL-T-9046J minimums are a tensile strength of 861 MPa and a yield strength (Rp0.2) of 827 MPa at 0 - 30°C, with at least 3 % elongation. The SAE heat treatment data give a solution treatment at 788 to 816 °C followed by ageing at 482 °C for 2 to 60 hours.
best_for: High-strength beta titanium sheet, strip and plate where AMS 4917 or MIL-T-9046J is specified
weakest_at: Wrought density, aged-condition strength and alloy-specific hazard data were not found in the sources held; the supplier powder figures disagree with the MIL minimums
identity:
formula: Beta titanium alloy Ti-13V-11Cr-3Al, titanium balance with nominal 13 % vanadium, 11 % chromium and 3 % aluminium by weight
source: efunda
where: 'Opening paragraph: composed, in weight percentage, of 13% Vanadium (V), 11% Chromium (Cr), 3% Aluminum (Al) and the base metal Titanium (Ti)'
designations:
- system: AMS
code: '4917'
note: sheet, strip and plate, solution heat treated
source: efunda
where: 'Opening paragraph: Other designations include MIL-T-9046 and AMS 4917'
- system: MIL
code: MIL-T-9046
note: titanium sheet, strip and plate
source: efunda
where: 'Opening paragraph: Other designations include MIL-T-9046 and AMS 4917'
- system: MIL
code: MIL-T-9046J
note: revision J, 1991, titanium and titanium alloy, sheet, strip and plate
source: totalmateria-mil
where: 'Chemical Composition section: MIL-T-9046J: 1991'
- system: Trade name
code: B120VCA
note: printed as B120VCA(Ti-13V-11Cr-3Al) in the 1962 design-data report
source: contrails
where: 'Record description: Four alloys were investigated: B120VCA(Ti-13V-11Cr-3Al)'
- system: Trade name
code: Ti-13-11-3
note: other name printed on the supplier page
source: samaterials
where: 'Product description: also called Ti-13-11-3'
tags:
environments: []
stresses: []
applications:
- structures
properties:
- benchmark: density
label: Density, spherical powder of Ti-13V-11Cr-3Al
value: 4.58
unit: g/cm3
scope: material
conditions:
form: spherical powder, supplier catalog DP4828 (listed as discontinued)
temperature: not stated
unit_in_source: 4.58g/cm 3
method: Value printed on a supplier product page
status: ground
note: Powder value, not a wrought sheet value. The Total Materia MIL page shows a placeholder for wrought density.
source: samaterials
where: Physical and Mechanical Properties list, Density
- benchmark: melting_point
label: Melting range, spherical powder of Ti-13V-11Cr-3Al
value: 1630
value_high: 1660
bound: range
unit: °C
scope: material
conditions:
form: spherical powder
pressure: not stated
unit_in_source: 1630~1660℃
method: Range printed on a supplier product page
status: ground
source: samaterials
where: Physical and Mechanical Properties list, Melting Point
- benchmark: ultimate_tensile_strength
label: Tensile strength Rm, MIL-T-9046J minimum
value: 861
bound: lower
unit: MPa
scope: material
conditions:
specification: 'MIL-T-9046J: 1991'
temperature: 0 - 30°C (column header as printed)
temper: not stated on the page
unit_in_source: ≥ 861 MPa
method: Minimum value printed in a Total Materia table for the MIL specification
status: ground
note: A minimum for the specification, not a typical value. The same page prints 950 MPa for the supplier powder.
source: totalmateria-mil
where: MIL Ti-13V-11Cr-3Al Mechanical Properties, Tensile Strength row, 0 - 30°C column
- benchmark: yield_strength
label: Yield strength Rp0.2, MIL-T-9046J minimum
value: 827
bound: lower
unit: MPa
scope: material
conditions:
specification: 'MIL-T-9046J: 1991'
temperature: 0 - 30°C (column header as printed)
temper: not stated on the page
unit_in_source: ≥ 827 MPa
method: Minimum value printed in a Total Materia table for the MIL specification
status: ground
source: totalmateria-mil
where: MIL Ti-13V-11Cr-3Al Mechanical Properties, Yield Strength Rp0.2 row, 0 - 30°C column
- benchmark: elongation
label: Elongation A, MIL-T-9046J minimum
value: 3
bound: lower
unit: '%'
scope: material
conditions:
specification: 'MIL-T-9046J: 1991'
temperature: 0 - 30°C (column header as printed)
unit_in_source: ≥ 3 %
method: Minimum value printed in a Total Materia table for the MIL specification
status: ground
source: totalmateria-mil
where: MIL Ti-13V-11Cr-3Al Mechanical Properties, Elongation A row
- benchmark: elastic_modulus
label: Modulus of elasticity, MIL Ti-13V-11Cr-3Al
value: 80
value_high: 130
bound: range
unit: GPa
scope: material
conditions:
specification: 'MIL-T-9046J: 1991'
temperature: not clearly stated in the extracted row
unit_in_source: 80 — 130 GPa
method: Range printed in a Total Materia physical properties table
status: ground
note: The same 80 to 130 GPa range is printed on the SAE page (totalmateria-sae).
source: totalmateria-mil
where: MIL Ti-13V-11Cr-3Al Physical Properties, Modulus of Elasticity row
- benchmark: thermal_conductivity
label: Thermal conductivity, MIL Ti-13V-11Cr-3Al
value: 8.044
unit: W/(m∙°C)
scope: material
conditions:
specification: 'MIL-T-9046J: 1991'
temperature: not stated
unit_in_source: 8.044 W/(m∙°C)
method: Value printed in a Total Materia physical properties table
status: ground
note: Disagrees with 6.7 W/(m*K) on the supplier powder page; both are kept side by side.
source: totalmateria-mil
where: MIL Ti-13V-11Cr-3Al Physical Properties, Thermal Conductivity row
- benchmark: ultimate_tensile_strength
label: Tensile strength (ultimate), spherical powder
value: 950
unit: MPa
scope: material
conditions:
form: spherical powder
temperature: not stated
temper: not stated
method: Value printed on a supplier product page
status: ground
note: Disagrees with the MIL minimum of 861 MPa; a supplier powder value with no temper or test temperature, not a specification minimum.
source: samaterials
where: Physical and Mechanical Properties list, Tensile Strength (Ultimate)
- benchmark: yield_strength
label: Yield strength, spherical powder
value: 850
unit: MPa
scope: material
conditions:
form: spherical powder
temperature: not stated
temper: not stated
method: Value printed on a supplier product page
status: ground
note: Disagrees with the MIL minimum of 827 MPa; a supplier powder value.
source: samaterials
where: Physical and Mechanical Properties list, Yield Strength
- benchmark: elongation
label: Elongation at break, spherical powder
value: 7
unit: '%'
scope: material
conditions:
form: spherical powder
temperature: not stated
temper: not stated
method: Value printed on a supplier product page
status: ground
source: samaterials
where: Physical and Mechanical Properties list, Elongation at break
- benchmark: elastic_modulus
label: Elastic modulus, spherical powder
value: 103
unit: GPa
scope: material
conditions:
form: spherical powder
temperature: not stated
method: Value printed on a supplier product page
status: ground
note: Falls inside the MIL range of 80 to 130 GPa; shown as a supplier value next to that range.
source: samaterials
where: Physical and Mechanical Properties list, Elastic Modulus
- benchmark: thermal_conductivity
label: Thermal conductivity, spherical powder
value: 6.7
unit: W/(m*K)
scope: material
conditions:
form: spherical powder
temperature: not stated
unit_in_source: 6.7W/(m*K)
method: Value printed on a supplier product page
status: ground
note: Disagrees with 8.044 W/(m∙°C) on the MIL page.
source: samaterials
where: Physical and Mechanical Properties list, Thermal Conductivity
- benchmark: specific_heat
label: Specific heat capacity, spherical powder
value: 515
unit: J/(kg*K)
scope: material
conditions:
form: spherical powder
temperature: not stated
unit_in_source: 515 J/(kg*K)
method: Value printed on a supplier product page
status: ground
source: samaterials
where: Physical and Mechanical Properties list, Specific Heat Capacity
- benchmark: vanadium_content
label: Vanadium content, supplier powder specification
value: 12.5
value_high: 14.5
bound: range
unit: '%'
scope: material
conditions:
form: spherical powder
basis: content as printed in the composition table
unit_in_source: Content (%)
method: Range printed in the composition table of a supplier product page
status: ground
note: The MIL page prints a placeholder for vanadium; this row is the only printed vanadium range read.
source: samaterials
where: Chemical Composition table, V column
- benchmark: chromium_content
label: Chromium content, supplier powder specification
value: 10
value_high: 12
bound: range
unit: '%'
scope: material
conditions:
form: spherical powder
basis: content as printed in the composition table
unit_in_source: 10.0~12.0
method: Range printed in the composition table of a supplier product page
status: ground
source: samaterials
where: Chemical Composition table, Cr column
- benchmark: aluminium_content
label: Aluminium content, supplier powder specification
value: 2.5
value_high: 3.5
bound: range
unit: '%'
scope: material
conditions:
form: spherical powder
basis: content as printed in the composition table
unit_in_source: 2.5~3.5
method: Range printed in the composition table of a supplier product page
status: ground
source: samaterials
where: Chemical Composition table, Al column
- benchmark: iron_content
label: Iron content, supplier powder specification
value: 0.35
bound: upper
unit: '%'
scope: material
conditions:
form: spherical powder
basis: single value printed, no range
unit_in_source: '0.35'
method: Value printed in the composition table of a supplier product page
status: ground
note: The table prints one value without a range or a label of maximum; it is shown as printed.
source: samaterials
where: Chemical Composition table, Fe column
- benchmark: carbon_content
label: Carbon content, supplier powder specification
value: 0.05
bound: upper
unit: '%'
scope: material
conditions:
form: spherical powder
basis: maximum, printed as less than or equal to
unit_in_source: ≤0.05
method: Limit printed in the composition table of a supplier product page
status: ground
source: samaterials
where: Chemical Composition table, C column
- benchmark: nitrogen_content
label: Nitrogen content, supplier powder specification
value: 0.08
bound: upper
unit: '%'
scope: material
conditions:
form: spherical powder
basis: maximum, printed as less than or equal to
unit_in_source: ≤0.08
method: Limit printed in the composition table of a supplier product page
status: ground
source: samaterials
where: Chemical Composition table, N column
- benchmark: hydrogen_content
label: Hydrogen content, supplier powder specification
value: 250
bound: upper
unit: ppm
scope: material
conditions:
form: spherical powder
basis: maximum
unit_in_source: 250ppm. Max.
method: Limit printed in the composition table of a supplier product page
status: ground
source: samaterials
where: Chemical Composition table, H column
- benchmark: solution_treatment_temperature
label: Solution treatment temperature, SAE heat treatment
value: 788
value_high: 816
bound: range
unit: °C
scope: material
conditions:
hold: within ±14°C (±25°F), then water quenched; sections may be air cooled
unit_in_source: 788 to 816°C (1450 to 1500°F)
method: Range printed in a Total Materia heat treatment section
status: ground
note: Process parameter with no canonical benchmark name; recorded under solution_treatment_temperature.
source: totalmateria-sae
where: Heat Treatments section, solution treatment
- benchmark: aging_temperature
label: Ageing temperature, SAE heat treatment
value: 482
unit: °C
scope: material
conditions:
tolerance: ±8°C (900°F ± 15°F)
hold: 2 to 60 hours, then air cooled
unit_in_source: 482°C ± 8°C (900°F ± 15°F)
method: Value printed in a Total Materia heat treatment section
status: ground
note: Process parameter with no canonical benchmark name; recorded under aging_temperature.
source: totalmateria-sae
where: Heat Treatments section, aging, first procedure
- benchmark: aging_time
label: Ageing time, SAE heat treatment
value: 2
value_high: 60
bound: range
unit: hours
scope: material
conditions:
temperature: 482°C ± 8°C
unit_in_source: 2 to 60 hour
method: Range printed in a Total Materia heat treatment section
status: ground
note: Process parameter with no canonical benchmark name; recorded under aging_time.
source: totalmateria-sae
where: Heat Treatments section, aging, first procedure, holding time
corrosion:
- environment: Seawater and general corrosion, supplier statement
headline: The powder supplier says the alloy has good corrosion resistance, including in seawater.
effect: Stanford Advanced Materials states that Ti-13-11-3 shows good corrosion resistance in the seawater environment, which suits marine use. The page gives no corrosion rate, test medium or exposure time.
rating: low
conditions:
basis: supplier wording only; no test data printed on the page
source: samaterials
where: Description and Applications text
risks:
hazards:
- text: PubChem's record for the element titanium (CID 23963) lists GHS hazard statements H228 (flammable solid), H250 (catches fire spontaneously if exposed to air) and H251 (self-heating; may catch fire) from a minority of company notifications, while most company reports say the element does not meet GHS hazard criteria. No safety data sheet for Ti-13V-11Cr-3Al was found, so this entry describes the element, not this alloy.
ghs:
- H228
- H250
- H251
source: pubchem-titanium
where: Safety and Hazards, GHS Classification (CID 23963)
failure_risks: []
side_effects: []
handling:
- text: 'Heat treat in two steps: solution treat at 788 to 816 °C and water quench, then age at 482 °C for 2 to 60 hours and air cool (SAE page).'
source: totalmateria-sae
where: Heat Treatments section
- text: Lighter sections may be air cooled after solution treatment instead of water quenched (SAE page).
source: totalmateria-sae
where: Heat Treatments section, solution treatment
- text: Check the governing specification, AMS 4917 or MIL-T-9046J, before use. The full texts of both were not read.
source: efunda
where: Opening paragraph, other designations
mitigations: []
uses:
- application: structures
device: Sheet, strip and plate in the solution-treated condition
example: The SAE listing for AMS4917E covers a titanium alloy of 13.5V - 11Cr - 3.0Al in the form of sheet, strip and plate, solution heat treated.
source: saemobilus
where: Title and Scope of AMS4917E
- application: structures
device: Aircraft components and structural parts
example: The powder supplier says the alloy is widely used in aerospace applications, such as aircraft components or structural parts.
source: samaterials
where: Applications paragraph
- application: structures
device: Spherical powder feedstock for additive manufacturing (3D printing)
example: The supplier offered the alloy as spherical powder, catalog DP4828, now discontinued, for making complex components by additive manufacturing.
source: samaterials
where: Product description and Applications paragraph
supply:
- subject: Titanium sponge metal (feedstock for titanium alloys)
abundance: USGS reports world sponge metal production of 370,000 tons in 2025 (estimated), after 380,000 tons in 2024. Sponge is the metal feedstock for alloys such as this one.
producers:
- country: China
year: 2025
- country: Japan
year: 2025
- country: Russia
year: 2025
- country: Kazakhstan
year: 2025
- country: Saudi Arabia
year: 2025
critical_lists: []
recycling: 'USGS: owing to limited responses from voluntary surveys, consumption data for titanium scrap metal for the titanium metal industry were withheld. The United States imported an estimated 44,000 tons of sponge in 2025 (estimated).'
substitutes:
- 'USGS: Aluminum, nickel, specialty steels, and zirconium alloys may be substituted for titanium for applications that require corrosion resistance.'
- 'USGS: In high-strength applications, titanium competes with aluminum, composites, intermetallics, steel, and superalloys.'
source: usgs-mcs2026-titanium
where: Salient Statistics, World Sponge Metal Production table (2025e), Recycling, Substitutes and Events, Trends, and Issues sections
documents:
- title: Stanford Advanced Materials, Titanium Alloy 13-11-3 Spherical Powder (Ti-13V-11Cr-3Al), catalog DP4828
type: datasheet
url: https://powder.samaterials.com/titanium-alloy-13-11-3-spherical-powder-ti-13v-11cr-3al.html
- title: 'Total Materia: MIL Ti-13V-11Cr-3Al (MIL-T-9046J) physical and mechanical properties'
type: database
url: https://www.totalmateria.com/en-us/material/3255813
- title: 'Total Materia: SAE Ti-13V-11Cr-3Al heat treatments and properties'
type: database
url: https://www.totalmateria.com/en-us/material/3210972
- title: 'eFunda: Ti-13V-11Cr-3Al wrought titanium alloy'
type: database
url: https://www.efunda.com/glossary/materials/alloys/materials--alloys--titanium_alloy--wrought--ti-13v-11cr-3al.cfm
- title: 'SAE: AMS4917E titanium alloy sheet, strip and plate, solution heat treated'
type: standard
url: https://saemobilus.sae.org/content/ams4917e
- title: Lockheed-Georgia, ASD TDR 62-335 Volume 3, design data for heat treated titanium alloy sheet (Illinois Institute of Technology record)
type: report
url: https://contrails.library.iit.edu/item/159100
year: 1962
- title: 'USGS Mineral Commodity Summaries 2026: Titanium and titanium dioxide'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-titanium.pdf
year: 2026
- title: 'PubChem: Titanium (CID 23963), GHS classification summary'
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/23963
gaps:
- No safety data sheet for the wrought alloy or its powder was found in the sources held. The only hazard entry is PubChem's record for the element titanium, which may not describe this alloy.
- No failure-mode or service-failure record for this alloy was found in the sources held.
- Aged-condition tensile, yield and elongation values for sheet, strip and plate were not found. The MIL figures are minimums with no stated temper. The 1962 Lockheed-Georgia report (ASD TDR 62-335 Volume 3) is an image-only PDF with no text layer, so its tables could not be read.
- The ASM Alloy Digest for Crucible B-120VCA is paywalled, and its visible text gives only a general stability statement without the test details needed to record a value.
- UNS R58010 is printed on the Total Materia SAE page, but that page marks the equivalence as Implicit, so it is not recorded as a designation.
- Wrought density and melting point were not found. The Total Materia MIL page shows a placeholder for density, and the only density and melting range are supplier powder values.
- The eFunda typical density, modulus and tensile figures apply to titanium alloys in general, not this grade, so they are not recorded.
- The MIL page prints a placeholder for vanadium, and the AMS 4917 composition table could not be read, so the vanadium limits come from the powder supplier only.
- The AMS 4917 title gives a vanadium figure that differs from the nominal vanadium content on eFunda. The difference is shown, not resolved.
- Specific heat, electrical resistivity and coefficient of thermal expansion for the wrought alloy were not found. Specific heat is recorded only for the supplier powder.
- Corrosion rate, outgassing and radiation data for this alloy in space conditions were not found in the sources held.
- The USGS titanium chapter read here does not print a critical-minerals listing for titanium, so critical_lists is empty.
- Country production shares for sponge are not calculated here. The producers list names the countries with printed 2025 sponge production.
- solution_treatment_temperature, aging_temperature and aging_time are not canonical benchmark names. No canonical name exists for these process steps.
sources:
samaterials:
title: Titanium Alloy 13-11-3 Spherical Powder (Ti-13V-11Cr-3Al), catalog DP4828, Stanford Advanced Materials
id: Catalog No. DP4828 (discontinued)
url: https://powder.samaterials.com/titanium-alloy-13-11-3-spherical-powder-ti-13v-11cr-3al.html
kind: datasheet
license: Supplier product page (cited, not reproduced)
totalmateria-mil:
title: 'Total Materia: MIL Ti-13V-11Cr-3Al, MIL-T-9046J: 1991 (physical, mechanical, composition)'
id: Total Materia material page 3255813
url: https://www.totalmateria.com/en-us/material/3255813
kind: database
license: Total Materia (cited, not reproduced); full data behind free registration
totalmateria-sae:
title: 'Total Materia: SAE Ti-13V-11Cr-3Al (heat treatments, physical and mechanical properties)'
id: Total Materia material page 3210972
url: https://www.totalmateria.com/en-us/material/3210972
kind: database
license: Total Materia (cited, not reproduced); full data behind free registration
efunda:
title: 'eFunda glossary: Ti-13V-11Cr-3Al wrought titanium alloy'
url: https://www.efunda.com/glossary/materials/alloys/materials--alloys--titanium_alloy--wrought--ti-13v-11cr-3al.cfm
kind: web
license: eFunda (cited, not reproduced)
saemobilus:
title: AMS4917E titanium alloy sheet, strip, and plate, 13.5V - 11Cr - 3.0Al, solution heat treated (SAE)
id: AMS4917E, revision E, reaffirmed
url: https://saemobilus.sae.org/content/ams4917e
kind: standard
license: SAE Mobilus listing (cited, not reproduced)
contrails:
title: ASD TDR 62-335 Volume 3, Determination of Design Data for Heat Treated Titanium Alloy Sheet, Tables of Data Collected (Lockheed-Georgia, 1962)
id: Illinois Institute of Technology record 159100
url: https://contrails.library.iit.edu/item/159100
year: 1962
kind: report
license: IIT Galvin Library record (cited, not reproduced)
usgs-mcs2026-titanium:
title: 'Mineral Commodity Summaries 2026: Titanium and titanium dioxide (USGS)'
id: USGS MCS 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-titanium.pdf
year: 2026
kind: report
license: Public domain (USGS)
pubchem-titanium:
title: 'PubChem: Titanium (CID 23963), Safety and Hazards, GHS Classification summary'
id: PubChem CID 23963
url: https://pubchem.ncbi.nlm.nih.gov/compound/23963
kind: database
license: PubChem (public domain, NCBI; cited, not reproduced)
license: CC-BY-4.0
updated: '2026-11-01'
review:
status: draft
method: assistant
checked_values: 23
unreachable: 0
caveats: 4
note: Values read by an AI assistant on 2026-11-01 from the pages named in each entry. Total Materia shows some values only behind a registration wall, so only printed values are recorded. The supplier powder and the MIL minimums disagree and are kept as separate rows. The 1962 report is image-only and was not used for values.
story:
recipe:
line: 'Ti-13V-11Cr-3Al is a titanium alloy: titanium is the balance, and vanadium, chromium and aluminium are the alloying additions. Supplier and specification pages print composition limits as percent by weight. The SAE page gives the heat treatment that follows melting and forming, a solution treatment and then ageing.'
parts:
- name: Titanium
symbol: Ti
role: Base metal, the balance of the alloy
share_note: balance (Bal.) as printed
source: samaterials
where: Chemical Composition table, Ti column
- name: Vanadium
symbol: V
role: Main alloying element
share_percent: 12.5
share_high: 14.5
source: samaterials
where: Chemical Composition table, V column
- name: Chromium
symbol: Cr
role: Alloying element
share_percent: 10
share_high: 12
source: samaterials
where: Chemical Composition table, Cr column
- name: Aluminium
symbol: Al
role: Alloying element
share_percent: 2.5
share_high: 3.5
source: samaterials
where: Chemical Composition table, Al column
- name: Iron
symbol: Fe
role: Impurity, as printed
share_percent: 0.35
share_note: printed as 0.35, no range
source: samaterials
where: Chemical Composition table, Fe column
- name: Carbon
symbol: C
role: Impurity limit
share_percent: 0.05
share_note: maximum, printed as ≤0.05
source: samaterials
where: Chemical Composition table, C column
- name: Nitrogen
symbol: 'N'
role: Impurity limit
share_percent: 0.08
share_note: maximum, printed as ≤0.08
source: samaterials
where: Chemical Composition table, N column
- name: Hydrogen
symbol: H
role: Impurity limit
share_note: maximum 250 ppm, as printed
source: samaterials
where: Chemical Composition table, H column
why: Ti-13V-11Cr-3Al is a beta titanium alloy with high strength for its weight. The MIL-T-9046J minimums are 861 MPa tensile and 827 MPa yield at 0 - 30°C, with at least 3 % elongation, and AMS 4917 covers the alloy as sheet, strip and plate in the solution-treated condition. A supplier of the alloy powder reports 950 MPa tensile and 850 MPa yield, a higher figure with no temper or test temperature stated, so the two sets of values are shown side by side rather than merged.
uses:
- where: Aircraft sheet, strip and plate
line: AMS 4917 covers this titanium alloy as sheet, strip and plate in the solution-treated condition, according to the SAE listing for AMS4917E.
- where: Aircraft components and structural parts
line: The powder supplier says the alloy is widely used in aerospace applications, such as aircraft components or structural parts.
- where: Additive manufacturing feedstock
line: The same supplier offered the alloy as spherical powder for making complex components by additive manufacturing. The catalog entry is now discontinued.
can_do:
- label: Tensile strength (specification minimum)
benchmark: ultimate_tensile_strength
value: 861 MPa minimum
line: Under MIL-T-9046J the tensile strength is at least 861 MPa at 0 - 30°C, per the Total Materia MIL table.
- label: Yield strength (specification minimum)
benchmark: yield_strength
value: 827 MPa minimum
line: The Rp0.2 yield strength is at least 827 MPa in the same table, with at least 3 % elongation.
- label: Powder density
benchmark: density
value: 4.58 g/cm3
line: The spherical powder has a density of 4.58 g/cm3 as printed by the supplier. A wrought density was not found.
- label: Melting range (powder)
benchmark: melting_point
value: 1630 to 1660 °C
line: The supplier powder prints a melting range of 1630 to 1660 °C.
- label: Ageing temperature
benchmark: aging_temperature
value: 482 °C
line: After solution treatment at 788 to 816 °C, the SAE page gives ageing at 482 °C for 2 to 60 hours.
- label: Elastic modulus
benchmark: elastic_modulus
value: 80 to 130 GPa
line: The modulus is printed as 80 to 130 GPa on the MIL and SAE Total Materia pages. The test temperature is not clear in the extracted row.
compare: 'The MIL-T-9046J minimums (861 MPa tensile and 827 MPa yield) are lower than the powder supplier''s stated values (950 MPa tensile and 850 MPa yield). A minimum is a floor a specification guarantees, while the supplier figure is a single product value with no temper or test temperature, so the two should not be ranked against each other. The thermal conductivity also differs by source: 8.044 W/(m∙°C) on the MIL page against 6.7 W/(m*K) for the powder.'
compare_rows:
- label: Tensile strength
benchmark: ultimate_tensile_strength
- label: Yield strength
benchmark: yield_strength
- label: Density
benchmark: density
handling:
- 'Heat treat in two steps: solution treat at 788 to 816 °C and water quench, then age at 482 °C for 2 to 60 hours and air cool.'
- Lighter sections may be air cooled after solution treatment instead of water quenched.
- Check the governing specification, AMS 4917 or MIL-T-9046J, before use. The full texts of both were not read.
good_for:
- Sheet, strip and plate for aircraft structures, where MIL-T-9046J sets minimum tensile and yield strengths.
- Age hardening after solution treatment, using the SAE heat treatment steps.
watch_out:
- The strength minimums carry no stated temper, so no aged-condition strength is recorded for sheet.
- The supplier powder and the MIL minimums disagree. Both are shown and neither is averaged.
- The wrought density and melting point were not found, so mass and melting data are powder values only.
- No hazard or failure data were found for this alloy.
verdict: Ti-13V-11Cr-3Al is a high-strength beta titanium alloy with MIL-T-9046J minimums of 861 MPa tensile and 827 MPa yield, and a published heat treatment of 788 to 816 °C solution treatment and 482 °C ageing. Its wrought density, aged-condition strength and alloy-specific hazard data are not in the sources held, and the supplier powder values differ from the specification minimums.
risk_groups:
- title: For people
lead: No safety data sheet for this alloy or its powder was found in the sources held. The only GHS data read is for the element titanium.
verdict: Element GHS data only
points:
- label: Powder
line: The supplier product page prints no hazard classification, and no safety data sheet for the alloy was found.
- title: If it fails
lead: The sources give specification minimums and supplier values, not failure records.
verdict: No failure records found
points:
- label: Strength floor
line: The MIL-T-9046J minimums are 861 MPa tensile and 827 MPa yield at 0 - 30°C. The supplier powder values of 950 MPa and 850 MPa carry no temper or test temperature.
- title: Handling and storage
points:
- label: Heat treatment
line: Solution treatment at 788 to 816 °C is followed by a water quench, and ageing at 482 °C for 2 to 60 hours, per the SAE page.
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.
Updated