Commercially pure titanium, Grade 2 (UNS R50400) CP Ti Grade 2

Unalloyed titanium, UNS R50400 (ASTM Grade 2): maximum limits on O, Fe, C, N and H, titanium the balance · CAS 7440-32-6

Also known as UNS R50400, ASTM B265, ASTM B348, ASTM B338, ASTM B337, ASTM B381 · 15 more

Commercially pure (CP) titanium Grade 2, UNS R50400, is unalloyed titanium with low limits on oxygen, iron, carbon, nitrogen and hydrogen.

14 sources · Updated 2026-10-24 · CC BY 4.0

Evidence level

2 of 5

Lab-measured

Strength

> 345 MPa

Ductility

> 20 %

Stiffness

103 GPa

Recipe, share of the weight

  • Ti balance (the rest)Titanium
  • O maximum 0.25 %Oxygen
  • Fe maximum 0.30 %Iron
  • C maximum 0.08 %Carbon
  • N maximum 0.03 %Nitrogen
  • H maximum 0.015 %Hydrogen

Best for

Seawater, brine and chloride service where corrosion resistance and formability matter more than strength (Alleima and Smiths datasheets)

Weakest at

Strength: 345 MPa minimum tensile, well below Ti-6Al-4V (see the Ti-6Al-4V profile). Crevice attack in hot seawater from about 80 °C (Pang and Blackwood 2016)

Risk at a glance

  • People Low. Solid: no class. Powder and swarf: flammable
  • If it fails High. Use in media titanium should not be used with
  • Corrosion Severe. Should not be used with these media.

Quick facts: CP Ti Grade 2

Key properties of CP Ti Grade 2
PropertyValueBasis
Density4.51 g/cm³1 sourced value
Yield strength275 to 352 MPa3 sourced values across conditions
Tensile strength345 to 483 MPa3 sourced values across conditions
Young's modulus103 GPa1 sourced value
Thermal conductivity22 W/(m·K)1 sourced value

What is the density of Commercially pure titanium, Grade 2 (UNS R50400)?

Commercially pure titanium, Grade 2 (UNS R50400) has a density of 4.51 g/cm³. The source and test conditions are listed in the properties table on this page.

What is the thermal conductivity of Commercially pure titanium, Grade 2 (UNS R50400)?

Commercially pure titanium, Grade 2 (UNS R50400) has a thermal conductivity of 22 W/(m·K). The source and test conditions are listed in the properties table on this page.

What is the yield strength of Commercially pure titanium, Grade 2 (UNS R50400)?

Commercially pure titanium, Grade 2 (UNS R50400) has a yield strength of 275 to 352 MPa. The range covers 3 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What is the tensile strength of Commercially pure titanium, Grade 2 (UNS R50400)?

Commercially pure titanium, Grade 2 (UNS R50400) has a tensile strength of 345 to 483 MPa. The range covers 3 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What is the Young's modulus of Commercially pure titanium, Grade 2 (UNS R50400)?

Commercially pure titanium, Grade 2 (UNS R50400) has a Young's modulus of 103 GPa. The source and test conditions are listed in the properties table on this page.

What are the other names and codes for Commercially pure titanium, Grade 2 (UNS R50400)?

Commercially pure titanium, Grade 2 (UNS R50400) is also written as UNS R50400, ASTM B265, ASTM B348, ASTM B338, ASTM B337, ASTM B381. Each code is printed in the source listed beside it in the designations table.

What is Commercially pure titanium, Grade 2 (UNS R50400) used for?

Uses recorded in the sources include Seawater-cooled heat exchanger and condenser tubing; Desalination pipe and reverse-osmosis pressure vessels; Aerospace hydraulic tubing (AMS 4943 annealed; AMS 4944 and 4945 cold worked and stress relieved).

Why it exists

Grade 2 is the most frequently employed unalloyed titanium grade (Smiths). It combines moderate strength with good ductility, formability and excellent weldability, and it resists seawater and chloride environments (Alleima). It is chosen when corrosion resistance and formability matter more than strength.

Where it's used

Seawater cooling and heat exchangers

Alleima lists tubing for heat exchangers and coolers that use seawater or chlorinated seawater as coolant, on oil platforms, in refineries and in chemical plants.

Desalination

Alleima lists tube and pipe for seawater transport, heat-exchanger tubing and pressure vessels for reverse-osmosis units.

Aerospace hydraulic tubing

Alleima lists AMS 4943 (annealed) and AMS 4944 and 4945 (cold worked and stress relieved) for hydraulic tubing in this grade.

Recipe

Unalloyed titanium, UNS R50400 (ASTM Grade 2): maximum limits on O, Fe, C, N and H, titanium the balance

Unalloyed titanium with no deliberate alloying additions. ASTM B265 limits the grade 2 composition to maximum oxygen, iron, carbon, nitrogen and hydrogen, with titanium as the balance. Wikipedia lists Grade 2 as the standard-oxygen unalloyed grade. Process routes are not described in the sources fetched for this profile.

What CP Ti Grade 2 is made of
IngredientShare of the weightWhat it does
Titanium Ti balance (the rest) Base metal. Gives the low density and the oxide-film corrosion resistance.
Oxygen O maximum 0.25 % Interstitial impurity with a maximum limit.
Iron Fe maximum 0.30 % Impurity with a maximum limit.
Carbon C maximum 0.08 % Interstitial impurity with a maximum limit.
Nitrogen N maximum 0.03 % Interstitial impurity with a maximum limit.
Hydrogen H maximum 0.015 % Interstitial impurity with a maximum limit.

Weight shares are as printed in the sources.

What it can do

Strength

> 345 MPa

measured

Minimum tensile strength 345 MPa and minimum 0.2 % yield strength 275 MPa for strip, sheet and plate (ASTM B265). Typical values in the Smiths datasheet are 483 MPa tensile and 352 MPa yield.

Ductility

> 20 %

measured

Minimum elongation 20 % (ASTM B265, 2 in or 50 mm gauge). Typical 28 % in the Smiths datasheet.

Stiffness

103 GPa

measured

Elastic modulus 103 GPa in tension, roughly one-half that of steel alloys (Alleima).

Corrosion

Resists seawater, brines and chlorides (Alleima and Titanium Industries). Crevice attack is not expected below 80 °C (Alleima).

How it compares

Grade 2 is the lower-strength titanium. The stronger alloy is [Ti-6Al-4V](/materials/ti-6al-4v). Grade 2 has a minimum tensile strength of 345 MPa and a minimum 0.2 % yield strength of 275 MPa (ASTM B265). Its elastic modulus of 103 GPa is roughly half that of steel alloys, and its density of 4.51 g/cm3 is 45 % less than ferrous alloys (Alleima).

The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.

Benchmarks
MeasurementCP Ti Grade 2Ti-6Al-4VTi-6Al-4V ELITi-3Al-2.5V (Grade 9)TiAlBeta 3Ti Grade 11Ti Gr 12CP Ti Grade 3CP Ti Grade 7Ti minor alloys
Capacity and energy
Charpy V-notch impact, minimum> 41 J1218 Jno data> 48 Jno datano datano datano data> 20 Jno datano data
Thermal behavior and safety
Thermal conductivity at room temperature22 W/(m·K)46.7 W/(m K)6.6 W/(m K)no datano datano data21.79 W/(m·K)19.02 W/(m·K)151.2 Btu-in/(hr·ft²·°F)21.79 W/m-K46.8 BTU-in/hr-ft2-°F
Physical and electrical
Density4.51 g/cm³14.43 g/cm³4.42 g/cm³4.48 g/cm³3.8 g/cm³5.07 g/cm³4.51 g/cm³4.51 g/cm³4.51 g/cm³4.51 g/cm³4.54 g/cm³
Hardness, typical160 HV1630 HRCno data15 HRCno data24 to 38 HRCno datano data200 HVno data24 to 38 HRC
Hardness, maximum< 92 HRB1730 HRCno data15 HRCno data24 to 38 HRCno datano data200 HVno data24 to 38 HRC
Other measurements
Elastic modulus (tension)103 GPa2113.8 GPa107 to 122 GPa91 GPa168 GPa82 GPa112 GPa103 GPa103 GPa112 GPa15000 ksi
Beta transus913 °C3995 °C966 °Cno datano data750 °C888 °C890 °C1690 °Fno data800 °C
Tensile strength, minimum (strip, sheet and plate)> 345 MPa5no data828 MPa> 620 MPa422 MPa1000 MPa> 240 MPa> 483 MPa> 450 MPa> 345 MPa< 175 ksi
Yield strength, 0.2 % offset, minimum (strip, sheet and plate)> 275 MPa6830 MPa759 MPa> 483 MPa326 MPa965 MPa> 138 MPa> 345 MPa> 380 MPa> 275 MPa< 186 ksi
Elongation, minimum (strip, sheet and plate)> 20 %710 %10 %> 15 %1.7 %7 %> 24 %> 18 %> 18 %> 20 %< 10 %
Tensile strength, minimum (seamless tube, ASTM B338)> 345 MPa8no data828 MPa> 620 MPa422 MPa1000 MPa> 240 MPa> 483 MPa> 450 MPa> 345 MPa< 175 ksi
Yield strength, minimum (seamless tube, ASTM B338)> 275 MPa9830 MPa759 MPa> 483 MPa326 MPa965 MPa> 138 MPa> 345 MPa> 380 MPa> 275 MPa< 186 ksi
Elongation, minimum (seamless tube, ASTM B338)> 20 %1010 %10 %> 15 %1.7 %7 %> 24 %> 18 %> 18 %> 20 %< 10 %
Reduction of area, minimum> 35 %11no data41.5 %no datano datano datano datano data> 35 %> 30 %no data
Yield strength, typical352 MPa13830 MPa759 MPa> 483 MPa326 MPa965 MPa> 138 MPa> 345 MPa> 380 MPa> 275 MPa< 186 ksi
Tensile strength, typical483 MPa14no data828 MPa> 620 MPa422 MPa1000 MPa> 240 MPa> 483 MPa> 450 MPa> 345 MPa< 175 ksi
Elongation, typical28 %1510 %10 %> 15 %1.7 %7 %> 24 %> 18 %> 18 %> 20 %< 10 %

Why choose it, and why not

Good for

  • Seawater cooling tubing and heat exchangers, where chloride resistance is needed (Alleima).
  • Forming and welding of sheet, plate and tube where ductility and weldability matter more than strength (Smiths).
  • Desalination pipe and reverse-osmosis pressure vessels (Alleima).

Watch out for

  • Crevice attack in chloride: none expected below 80 °C, but Grade 2 crevice-corroded at 80 °C in near-anaerobic seawater (Alleima; Pang and Blackwood).
  • Lower strength than Ti-6Al-4V: 345 MPa minimum tensile (see the Ti-6Al-4V profile).
  • Do not use with strong reducing acids, fluoride solutions, pure oxygen or anhydrous chlorine (Alleima).
  • Springback is about twice that of stainless steel in bending (Alleima).
  • Powder and swarf are a flammable-solid fire hazard (PubChem).

CP titanium Grade 2 is the corrosion-resistant, formable titanium grade for seawater and chloride service. Its strength is modest, with a 345 MPa minimum tensile strength, so it is not a structural alloy like Ti-6Al-4V. Its limits are crevice attack in hot seawater and the media it should not be used in.

Technical details

For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.

Other names and standards

The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.

Other names and standards
SystemCodes
UNSR50400
ASTMB265 (strip, sheet and plate), B348 (bars and billets), B338 (seamless and welded tube), B337 (seamless and welded pipe), B381 (forgings), B861 (seamless pipe), B862 (welded pipe), B863 (wire and rod), F67 (sheet, plate and bar)
ASMESB-265 (strip, sheet and plate), SB-348 (bars and billets), SB338 (seamless and welded tube), B862 (welded pipe)
AMS4902 (sheet and plate), 4943 (aerospace hydraulic tubing, annealed), 4944 (aerospace hydraulic tubing, cold worked and stress relieved), 4945 (aerospace hydraulic tubing, cold worked and stress relieved), 4951 (commercially pure weld wire)
NameTitanium Grade 2
Trade nameTi Grade 2

Notes

The method, full conditions and any caveat for the numbered rows above.

Notes for the numbered rows
#MeasurementMethodConditionsCaveat
1DensityPrinted in the Physical properties section of the Alleima Ti Grade 2 datasheet, which also says the density is 45 % less than ferrous alloys. The Smiths CP Grade 2 datasheet also gives 4.51 g/cc.form seamless tube and pipe (the Alleima datasheet product)condition not stated; alloy density—
2Elastic modulus (tension)Printed in the Elastic modulus section of the Alleima datasheet, tension row (15.0 x 10^6 psi and 103 GPa). The Smiths datasheet prints the same 103 GPa as a typical value.form seamless tube and pipeloading tensioncondition not stated—
3Beta transusPrinted as 1675F (913C) in the Physical properties section of the Alleima datasheet. The Celsius value is used.form seamless tube and pipecondition not statedprinted as 1675 F—
4Thermal conductivity at room temperaturePrinted as 22 W/m'C (12.7 BTU) at RT in the Thermal Conductivity section of the Alleima datasheet. The number is the same in W/(m·K) because the degree and kelvin intervals are equal.form seamless tube and pipetemperature room temperature (printed RT)unit in source W/m'C (the degree sign is printed as an apostrophe)—
5Tensile strength, minimum (strip, sheet and plate)Minimum in Table 1 (Tensile Requirements) of the ASTM B265-08b copy, with 50 ksi printed beside 345 MPa.form strip, sheet and plate (ASTM B265 product)condition as specified for Grade 2 in ASTM B265-08b Table 1minimum yes—
6Yield strength, 0.2 % offset, minimum (strip, sheet and plate)Minimum in Table 1 of the ASTM B265-08b copy, with 40 ksi printed beside 275 MPa. The same row prints a maximum of 450 MPa (65 ksi), which is not recorded here.form strip, sheet and plate (ASTM B265 product)offset 0.2 %minimum yes—
7Elongation, minimum (strip, sheet and plate)Minimum elongation in Table 1 of the ASTM B265-08b copy.form strip, sheet and plate (ASTM B265 product)gauge 2 in or 50 mmminimum yes—
8Tensile strength, minimum (seamless tube, ASTM B338)Printed as Min 50 ksi and 345 MPa in the tensile properties table for Grade 2 to ASTM B338 in the Alleima datasheet.form seamless tube and pipe (ASTM B338 Grade 2)condition cold reduced or cold reduced and annealed, as suppliedminimum yes—
9Yield strength, minimum (seamless tube, ASTM B338)Printed as Min 40 ksi and 275 MPa in the same Alleima table.form seamless tube and pipe (ASTM B338 Grade 2)condition cold reduced or cold reduced and annealed, as suppliedoffset not printed in the tableminimum yes—
10Elongation, minimum (seamless tube, ASTM B338)Printed as Elongation 2 in, Min 20 % in the same Alleima table.form seamless tube and pipe (ASTM B338 Grade 2)gauge 2 incondition cold reduced or cold reduced and annealed, as suppliedminimum yes—
11Reduction of area, minimumPrinted in the Mechanical Properties table of the Smiths CP Grade 2 datasheet. reduction_of_area is not in the canonical list, so a snake_case name is used (see gaps).form CP Grade 2 product (datasheet covers bar, wire, strip, sheet, plate, foil, forgings and pipe or tube)condition minimum as printed; no separate condition givenminimum yes—
12Charpy V-notch impact, minimumPrinted in the Mechanical Properties table of the Smiths CP Grade 2 datasheet. impact_energy is a snake_case name (see gaps).form CP Grade 2 product (datasheet product range)test Charpy V-notchminimum yes—
13Yield strength, typicalPrinted as 0.2% PS, typical 352 MPa in the Smiths datasheet. The datasheet minimum of 276 MPa is not used here; the ASTM minimum of 275 MPa is recorded instead.form CP Grade 2 product (datasheet product range)offset 0.2 %basis typical, not a minimum—
14Tensile strength, typicalPrinted in the UTS row, typical column, of the Smiths CP Grade 2 datasheet.form CP Grade 2 product (datasheet product range)basis typical, not a minimum—
15Elongation, typicalPrinted in the Elongation on 2 in row, typical column, of the Smiths CP Grade 2 datasheet.form CP Grade 2 product (datasheet product range)gauge 2 inbasis typical, not a minimum—
16Hardness, typicalPrinted as Hardness HV, typical 160, in the Smiths CP Grade 2 datasheet.form CP Grade 2 product (datasheet product range)basis typical—
17Hardness, maximumPrinted as 92 HRB max. in the Hardness section of the Alleima datasheet.form seamless tube and pipecondition supplied as cold reduced or cold reduced and annealed—

Corrosion and compatibility

What happens when it meets other materials and environments.

Corrosion and compatibility
EnvironmentConcernWhat happens
Seawater and brines, general corrosion low Excellent resistance to general corrosion in seawater and brines.1
Chlorides and common salt solutions, pH 3 to 12 low Resists most natural waters and common salt solutions, including chlorides, from pH 3 to 12.2
Crevice corrosion below 80 °C low No crevice corrosion expected below 80 °C at any pH, even in super-chlorinated water.3
Near-anaerobic seawater at 80 °C and above moderate Grade 2 suffers crevice corrosion at 80 °C in near-anaerobic seawater.4
Hot chloride solutions and seawater (stress corrosion cracking) low Excellent resistance to stress corrosion cracking; immune in seawater.5
Flowing seawater (erosion) low Negligible erosion in flowing seawater up to 40 m/s.6
Galvanic coupling moderate Titanium is normally the cathode and can accelerate corrosion of a coupled metal.7
Strong reducing acids, fluoride solutions, pure oxygen, anhydrous chlorine severe Should not be used with these media.8
Hydrogen pickup in seawater low No significant hydrogen absorption in seawater unless three conditions are met together.9
General corrosion (product description) low Outstanding corrosion resistance, with strength similar to austenitic stainless steels.10
Corrosion details
#EnvironmentDetailsTest conditions
1 Seawater and brines, general corrosion Alleima says CP titanium has excellent resistance to general corrosion in seawater, and lists seawater and brines among the media where it shows good corrosion resistance. The datasheet prints no test conditions. basis manufacturer statement; no test conditions printedform seamless tube and pipe (Alleima datasheet)
2 Chlorides and common salt solutions, pH 3 to 12 Titanium Industries says titanium alloys are usually expected to resist most natural waters and common salt solutions, including chlorides, in a pH range of 3 to 12. The statement is for titanium alloys in general, not a Grade 2 test. basis general statement for titanium alloys; no Grade 2 test conditionspH 3 to 12
3 Crevice corrosion below 80 °C Alleima says CP titanium will not exhibit crevice corrosion at temperatures under 80 °C regardless of pH, even under super-chlorinated conditions, and resists crevice attack in salt solutions better than stainless steels. temperature below 80 °CpH anychlorides super-chlorinated
4 Near-anaerobic seawater at 80 °C and above Pang and Blackwood tested Grades 2, 5 and 7 in near-anaerobic seawater (below 1 ppm oxygen) up to 200 °C, with and without CO2. The abstract says Grade 2 suffers crevice corrosion at 80 °C and Grade 5 at 200 °C. electrolyte seawater, near-anaerobic (below 1 ppm oxygen)temperature up to 200 °C; crevice attack for Grade 2 at 80 °CCO2 tested with and without CO2
5 Hot chloride solutions and seawater (stress corrosion cracking) Alleima says Grade 2 shows excellent resistance to stress corrosion cracking in hot chloride solutions and is immune to SCC in seawater. Titanium Industries says titanium does not show the same susceptibility to chloride stress corrosion as stainless steel. basis manufacturer statements; no test conditions printed
6 Flowing seawater (erosion) Alleima says titanium shows excellent resistance to erosion in flowing seawater up to 130 ft/s (40 m/s), with negligible effect. Sand has only a small effect. velocity up to 40 m/s (130 ft/s)medium flowing seawater
7 Galvanic coupling Alleima says titanium is near the noble end of the galvanic series and normally acts as the cathode. It is not itself affected by galvanic corrosion, but it can accelerate corrosion of the metal it is coupled to. basis galvanic series position; no test conditions printed
8 Strong reducing acids, fluoride solutions, pure oxygen, anhydrous chlorine Alleima says titanium should not be used with strong reducing acids, fluoride solutions, pure oxygen or anhydrous chlorine. The datasheet prints no concentrations. basis manufacturer advice; no concentrations printed
9 Hydrogen pickup in seawater Alleima says hydrogen absorption normally occurs only when the pH is below 3 or above 12, the temperature is above 80 °C, and a hydrogen source such as a galvanic couple or impressed current is present. basis conditional; all three conditions must be met
10 General corrosion (product description) Austral Wright describes Grade 2 as a commercially pure titanium grade with outstanding corrosion resistance and useful strength, similar to austenitic stainless steels. The description prints no test conditions. basis product description; no test conditions

Risks and side effects

Hazards to people, what happens when a cell overheats, and how the material is handled and stored.

For people

The solid metal is not hazard-classed in the sources fetched here. PubChem gives titanium a flammable-solid classification (H228), which applies to powder and swarf.

Solid metal
Sheet, plate, bar and tube are covered by the Smiths and Alleima datasheets, which carry no hazard classification.
Powder and swarf
PubChem gives H228 (flammable solid) from aggregated reports. Treat powder and swarf as a fire hazard.

Test details
The original wording and numbers from the sources, for readers who want them.

Failure risks

Failure risks
FailureTrigger and consequence
Crevice corrosion in hot seawater from 80 °Cmoderate severityTight crevices in seawater at 80 °C and aboveLocal attack in the crevice; Pang and Blackwood report it for Grade 2 at 80 °C in near-anaerobic seawater
Use in media titanium should not be used withhigh severityStrong reducing acids, fluoride solutions, pure oxygen or anhydrous chlorineAlleima advises against these media; no concentrations are printed
Galvanic coupling to a less noble metalmoderate severityElectrical contact with a less noble metal in an electrolyteTitanium acts as the cathode and accelerates corrosion of the coupled metal
Galling of the tube bore and springback in bendinglow severityBending thin-walled tube or using a tight radius without a well-lubricated mandrelGalling of the ID surface; springback about twice that of stainless steel

Handling and storage

  • Weldability is excellent. Specified bend radius is 2.0 times thickness for sections under 0.070 in and 2.5 times thickness above that. Welded bend radius is 3.0 times thickness at minimum.
  • Welding is regularly done by TIG. Inert gas shielding must cover both OD and ID of tube, the surface must be free of grease and oil, a low heat input is used, and no post-weld heat treatment is normally performed.
  • Bend thin-walled tube with a well-lubricated mandrel to prevent galling of the ID surface. Allow for springback about twice that of stainless steel.
  • Machining: use low cutting speeds and high feed rates, large volumes of coolant, sharp tools, and never stop feeding while the tool is in contact with the workpiece.
  • Do not use with strong reducing acids, fluoride solutions, pure oxygen or anhydrous chlorine.

Supply and geography

How common the raw materials are and where they come from.

Titanium sponge (feedstock for titanium mill products)

The USGS 2026 titanium summary fetched for this profile gives no crustal abundance or resource tonnage. It refers to a separate titanium mineral concentrates chapter.

Top producers (2025)
China 70.3%, Japan 14.3%, Russia 6.8%, Kazakhstan 4.3%, Saudi Arabia 3.2%