Aluminium alloy 5251 AlMg2
AlMg2Mn0.3 (aluminium with 1.70 to 2.40 wt% Mg, 0.10 to 0.50 wt% Mn, up to 0.50 wt% Fe, up to 0.40 wt% Si, balance Al
Also known as UNS A95251, EN 3.3525, EN name EN AW-5251, DIN AlMg2Mn0.3, BS NS4, ISO AlMg2
Aluminium alloy 5251 (EN AW-5251, AlMg2Mn0.3) is a non-heat-treatable wrought aluminium-magnesium alloy with 1.70 to 2.40 wt% magnesium.
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Carry heat
138 W/(m·K)
Strength when soft
60 MPa proof stress (O)
Strength after cold work
120 MPa proof stress (H22)
Weight
2.69 g/cm3
Melting
605 to 650 °C
Recipe, share of the weight
- Al not statedAluminium
- Mg not statedMagnesium
- Mn not statedManganese
Best for
Welded marine and sheet-metal structures where seawater corrosion resistance and weldability matter more than peak strength, at 2.69 g/cm3
Weakest at
Strength compared with heat-treatable alloys: H22 minimum proof stress is 120 MPa, and a good weld reaches only about 160 MPa (Smith)
Risk at a glance
- People Low. Low as solid sheet, higher for dust and fume
- If it fails Moderate. Strength loss in welds of strain-hardened tempers
- Corrosion Low. 5251 is described as highly corrosion resistant in marine environments.
Quick facts: AlMg2
| Property | Value | Basis |
|---|---|---|
| Density | 2.68 to 2.69 g/cm³ | 2 sourced values across conditions |
| Yield strength | at least 60 MPa | 4 sourced values across conditions |
| Tensile strength | 160 to 285 MPa | 4 sourced values across conditions |
| Young's modulus | 70 GPa | 1 sourced value |
| Thermal conductivity | 138 to 149 W/(m·K) | 2 sourced values across conditions |
| Thermal expansion (CTE) | 23.8 ppm/K | 1 sourced value |
| Melting point | 605 to 650 °C | 1 sourced value |
| Specific heat | 898 J/(kg·K) | 1 sourced value |
| Electrical resistivity | 50 nΩ·m | 1 sourced value |
What is the density of Aluminium alloy 5251 (AlMg2)?
Aluminium alloy 5251 (AlMg2) has a density of 2.68 to 2.69 g/cm³. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the thermal conductivity of Aluminium alloy 5251 (AlMg2)?
Aluminium alloy 5251 (AlMg2) has a thermal conductivity of 138 to 149 W/(m·K). The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the coefficient of thermal expansion of Aluminium alloy 5251 (AlMg2)?
Aluminium alloy 5251 (AlMg2) has a coefficient of thermal expansion of 23.8 ppm/K. The source and test conditions are listed in the properties table on this page.
What is the melting point of Aluminium alloy 5251 (AlMg2)?
Aluminium alloy 5251 (AlMg2) has a melting point of 605 to 650 °C. The source and test conditions are listed in the properties table on this page.
What is the yield strength of Aluminium alloy 5251 (AlMg2)?
Aluminium alloy 5251 (AlMg2) has a yield strength of at least 60 MPa. The range covers 4 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What are the other names and codes for Aluminium alloy 5251 (AlMg2)?
Aluminium alloy 5251 (AlMg2) is also written as UNS A95251, EN 3.3525, EN name EN AW-5251, DIN AlMg2Mn0.3, BS NS4, ISO AlMg2. Each code is printed in the source listed beside it in the designations table.
What is Aluminium alloy 5251 (AlMg2) used for?
Uses recorded in the sources include Boats, marine structures, panelling and vehicle panels; Aircraft fuel tanks and oxygen cylinders (supplier claim); Satellite shells and missile structures (supplier claim).
Why it exists
Aluminium alloy 5251 is chosen for sheet work that has to bend and weld and resist seawater, with more strength than pure aluminium. Its magnesium content is low enough that Atlas says it avoids the stress corrosion cracking of alloys with more than about 3.5 % Mg. At 2.69 g/cm3 (Aalco H22) it is light compared with steel. Suppliers list it for boats, panelling, pressure work, fuel tanks and, in one supplier's claim, satellite shells.
Where it's used
Marine and sheet metal work
Aalco lists boats, panelling and pressings, marine structures, vehicle panels and containers as typical uses.
Aircraft and spacecraft parts (supplier claims)
Chalco says 5251 can be used for aircraft fuselage shells, fuel tanks and oxygen cylinders, and that it has been used for satellite shells and missile structures. These are supplier claims, and no qualification data was opened.
Heat transfer and pressure work
Smith lists heat transfer devices, pressure vessels, boiler making and chemical industry work among typical uses of its 5251 sheet.
Recipe
AlMg2Mn0.3 (aluminium with 1.70 to 2.40 wt% Mg, 0.10 to 0.50 wt% Mn, up to 0.50 wt% Fe, up to 0.40 wt% Si, balance Al; limits as printed to BS EN 573-3 in the Aalco H22 datasheet)
Wrought aluminium alloy AlMg2Mn0.3, with magnesium as the main alloying element and manganese as the second (Atlas describes it as a 2 % magnesium, 0.3 % manganese alloy). It is not heat-treatable; strength comes from cold rolling into the H tempers and partial annealing (Atlas). Composition limits are from Aalco (BS EN 573-3). The datasheets do not describe the casting route.
| Ingredient | Share of the weight | What it does |
|---|---|---|
| Aluminium Al | not stated | Matrix metal. Aalco prints aluminium as the balance of the composition. |
| Magnesium Mg | not stated | Main alloying element; the alloy is non-heat-treatable and its strength comes from cold work (Atlas). |
| Manganese Mn | not stated | Alloying element, printed with magnesium in the designation AlMg2Mn0.3 (Modulus Metal, DIN 1725-1). |
Weight shares are as printed in the sources.
What it can do
Carry heat
138 W/(m·K)
measured
Atlas gives 138 W/(m·K) at 25 °C as a typical value. Smith prints 149 and Aalco prints 134, both without a stated temperature, so the datasheets differ.
Strength when soft
60 MPa proof stress (O)
measured
The O temper has a minimum proof stress of 60 MPa and a tensile strength of 160 to 200 MPa, per the BS EN 485-2 values in the AZoM table.
Strength after cold work
120 MPa proof stress (H22)
measured
H22 has a minimum proof stress of 120 MPa and a tensile strength of 190 to 230 MPa. H24 has 140 MPa and 210 to 250 MPa.
Weight
2.69 g/cm3
measured
Density is 2.69 g/cm3 in the Aalco datasheet. Atlas gives 2680 kg/m3 as a typical value.
Melting
605 to 650 °C
measured
Euralliage gives a solidus of 605 °C and a liquidus of 650 °C.
Expansion
23.8 µm/m/°C
measured
Atlas gives a mean thermal expansion of 23.8 µm/m/°C between 20 and 100 °C.
How it compares
Atlas says the specified yield strength of this alloy in the H32 and H34 tempers is substantially lower than that of its sister alloy in the same tempers, so substitution needs care. The USGS says copper can replace aluminium in electrical and heat-exchange applications, so the two metals compete in conductors and heat exchangers.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | AlMg2 | 6061 | 7075-T6 | 2024 | 5052 | 5XXX | 2195 (Al-Cu-Li) | Al | 1050 | 2011 | 2014 | 2017 | 2017A | 2219 | 2319 | 2618A | 3003 | 3103 | 4047 | 5019 | 5056 | 5083 | AlMg3 | 6013 | 6063 | 6082 | 6101 | AA7050 | AA8011 | Au-Al IMCs | Al master alloys |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Thermal behavior and safety | |||||||||||||||||||||||||||||||
| Melting range (solidus to liquidus), alloy 5251 | 605 to 650 °C3 | no data | 532 °C | no data | 607.2 to 649 °C | no data | 1020 degF | 660 °C | 645 to 657 °C | 540 °C | 535 °C | 510 °C | 510 °C | 543 °C | 543 to 643 °C | 549 °C | 655 °C | 655 °C | 1068 to 1080 °F | 575 to 630 °C | 565 to 640 °C | 570 °C | 590 to 645 °C | 579 °C | 600 °C | 575 °C | 1090 °F | 490 °C | 640 to 655 °C | no data | 880 °C |
| Thermal conductivity at 25 °C, alloy 5251 (typical values)Typical value printed in a datasheet | 138 W/(m·K)5 | 167 W/(m·K) | 130 W/m·K | 121 W/m-K | 138 W/m-K | 138 W/(m·K) | no data | 220 W/(m·K) | 229 W/m.K | 140 W/m.K | 138 W/(m·K) | 140 W/m.K | 140 W/m.K | 130 W.m/m2.°C | no data | 147 W/m.K | 190 W/m.K | 160 W/m.K | no data | 110 to 140 W/(m·K) | 109 to 117 W/(m·K) | 121 W/(m·K) | 140 to 160 W/(m·K) | 164 W/(m·K) | 200 W/(m·K) | 180 W/(m·K) | no data | 154 W/(m·K) | 210 to 220 W/(m·K) | no data | no data |
| Thermal conductivity, alloy 5251 (Smith typical values) | 149 W/(m·K)6 | 167 W/(m·K) | 130 W/m·K | 121 W/m-K | 138 W/m-K | 138 W/(m·K) | no data | 220 W/(m·K) | 229 W/m.K | 140 W/m.K | 138 W/(m·K) | 140 W/m.K | 140 W/m.K | 130 W.m/m2.°C | no data | 147 W/m.K | 190 W/m.K | 160 W/m.K | no data | 110 to 140 W/(m·K) | 109 to 117 W/(m·K) | 121 W/(m·K) | 140 to 160 W/(m·K) | 164 W/(m·K) | 200 W/(m·K) | 180 W/(m·K) | no data | 154 W/(m·K) | 210 to 220 W/(m·K) | no data | no data |
| Specific heat capacity, alloy 5251 | 898 J/(kg·K)8 | no data | 960 J/kg·K | 0.875 J/g-°C | no data | no data | no data | 900 J/(kg·K) | no data | no data | no data | 0.88 J/(g·°C) | 0.88 J/g-°C | 0.86 J/g.°C | no data | no data | no data | no data | no data | 904 J/(kg·K) | no data | no data | 900 J/(kg·K) | no data | no data | 896 J/(kg·K) | no data | 0.86 J/g°C | no data | no data | no data |
| Physical and electrical | |||||||||||||||||||||||||||||||
| Density, alloy 5251 (sheet and plate, H22 datasheet) | 2.69 g/cm³1 | 2.7 g/cm³ | 2.8 Mg/m3 | 2.78 g/cc | 2.68 g/cc | 2.68 g/cm³ | 0.096 lb/in3 | 2.7 g/cm³ | 2.71 g/cm³ | 2.82 g/cm³ | 2.82 g/cm³ | 2.79 g/cm³ | 2.79 g/cm³ | 2.84 g/cm³ | 2.84 g/cm³ | 2.76 g/cm³ | 2.73 g/cm³ | 2.73 g/cm³ | 2.65 g/cm³ | 2.64 g/cm³ | 2.64 g/cm³ | 2.65 g/cm³ | 2.67 g/cm³ | 2.71 g/cm³ | 2700 kg/m3 | 2.7 g/cm³ | 0.097 lb/cu.in | 2.83 g/cm³ | 2.71 g/cm³ | no data | no data |
| Density, alloy 5251 (typical values) | 2680 kg/m32 | 2.7 g/cm³ | 2.8 Mg/m3 | 2.78 g/cc | 2.68 g/cc | 2.68 g/cm³ | 0.096 lb/in3 | 2.7 g/cm³ | 2.71 g/cm³ | 2.82 g/cm³ | 2.82 g/cm³ | 2.79 g/cm³ | 2.79 g/cm³ | 2.84 g/cm³ | 2.84 g/cm³ | 2.76 g/cm³ | 2.73 g/cm³ | 2.73 g/cm³ | 2.65 g/cm³ | 2.64 g/cm³ | 2.64 g/cm³ | 2.65 g/cm³ | 2.67 g/cm³ | 2.71 g/cm³ | 2700 kg/m3 | 2.7 g/cm³ | 0.097 lb/cu.in | 2.83 g/cm³ | 2.71 g/cm³ | no data | no data |
| Electrical resistivity, alloy 5251 (typical values)Typical value printed in a datasheet | 50 nΩ·m9 | 4 µΩ·cm | 5.2 µΩ·cm | 5.82 µΩ·cm | no data | 5.8 µΩ·cm | no data | 2.646 µΩ·cm | no data | no data | 0.045 µΩ·m | no data | no data | 5.7 μΩ.cm²/cm | no data | no data | no data | no data | no data | 0.0526 to 0.0667 Ω·mm²/m | 5.88×10^-8 to 6.25×10^-8 Ω·m | 0.058 µΩ·m | no data | no data | 0.35 µΩ·m | 0.038 µΩ·m | no data | no data | 2.86×10^-8 to 2.94×10^-8 Ω·m | no data | no data |
| Electrical conductivity, alloy 5251 (% IACS) | 39.4 % IACS10 | no data | no data | no data | no data | 29 % IACS | no data | no data | 58.4 % IACS | no data | no data | no data | no data | 17.4 x10^6 S/m | no data | no data | no data | no data | 41 % IACS | no data | no data | no data | 20 to 23 m/(Ω·mm²) | no data | no data | 42 %IACS | 57 % IACS | > 23 MS/m | 3.4×10^7 to 3.5×10^7 S/m | no data | no data |
| Other measurements | |||||||||||||||||||||||||||||||
| Modulus of elasticity, alloy 5251 | 70 GPa4 | 68.9 GPa | 71 GPa | 73.1 GPa | 70.3 GPa | 70.3 GPa | 11 MSI | 69 GPa | 69000 MPa | 70 GPa | 71 GPa | 72 GPa | 72 GPa | 73.8 x10^3 N/mm2 | no data | 71 GPa | 69.5 GPa | 69.5 GPa | no data | 70 GPa | 71 GPa | 72 GPa | 70 GPa | 71 GPa | 69.5 GPa | 70 GPa | no data | 71.5 GPa | 70 GPa | no data | no data |
| Mean coefficient of thermal expansion, 20 to 100 °C, alloy 5251Typical value printed in a datasheet | 23.8 µm/m/°C7 | 23.6 ppm/K | 23.4 µm/m·K | 23.2 ppm/K | 24.8 µm/m-°C | 24 ppm/K | no data | 22.5 ppm/K | 23.5 x10-6/K | 21.4 µm/m.°C | 23 ppm/K | 22.9 µm/(m·°C) | 22.9 µm/m.°C | 22.5 x10^-6 m/m.°C | no data | 21.6 µm/m°C | 23.1 ppm/K | 23.1 x10-6/K | no data | no data | 2.41×10^-5 1/K | 25 ppm/K | 23.9 ppm/K | 21.7 µm/m°C | 23.5 ppm/K | 23.1 ppm/K | no data | 23.5 ppm/K | 2.35×10^-5 1/K | no data | no data |
| Yield strength Rp0.2 minimum, H22 temper | > 120 MPa11 | 276 MPa | 503 MPa | 324 MPa | 13 ksi | 193 MPa | 74 ksi | 29 MPa | > 85 MPa | 140 MPa | > 400 MPa | 276 MPa | 276 MPa | > 50 ksi | 70 MPa | 350 MPa | 50 MPa | > 110 MPa | 55 MPa | no data | no data | > 125 MPa | > 80 MPa | 350 MPa | 21 ksi | > 255 MPa | 28000 psi | > 414 MPa | no data | no data | no data |
| Tensile strength, H22 temper | 190 to 230 MPa12 | 310 MPa | 572 MPa | 469 MPa | 28 ksi | 228 MPa | 80 ksi | 88 MPa | 105 to 145 MPa | 300 MPa | > 460 MPa | 427 MPa | 427 MPa | > 62 ksi | 160 MPa | 420 MPa | 110 MPa | > 140 MPa | 124 MPa | 270 to 350 MPa | 300 MPa | 275 to 350 MPa | 190 to 260 MPa | 410 MPa | 27 ksi | > 300 MPa | 32000 psi | > 483 MPa | 180 to 195 MPa | no data | no data |
| Yield strength Rp0.2 minimum, H24 temper | > 140 MPa13 | 276 MPa | 503 MPa | 324 MPa | 13 ksi | 193 MPa | 74 ksi | 29 MPa | > 85 MPa | 140 MPa | > 400 MPa | 276 MPa | 276 MPa | > 50 ksi | 70 MPa | 350 MPa | 50 MPa | > 110 MPa | 55 MPa | no data | no data | > 125 MPa | > 80 MPa | 350 MPa | 21 ksi | > 255 MPa | 28000 psi | > 414 MPa | no data | no data | no data |
| Tensile strength, H24 temper | 210 to 250 MPa14 | 310 MPa | 572 MPa | 469 MPa | 28 ksi | 228 MPa | 80 ksi | 88 MPa | 105 to 145 MPa | 300 MPa | > 460 MPa | 427 MPa | 427 MPa | > 62 ksi | 160 MPa | 420 MPa | 110 MPa | > 140 MPa | 124 MPa | 270 to 350 MPa | 300 MPa | 275 to 350 MPa | 190 to 260 MPa | 410 MPa | 27 ksi | > 300 MPa | 32000 psi | > 483 MPa | 180 to 195 MPa | no data | no data |
| Yield strength Rp0.2 minimum, O (annealed) temper | > 60 MPa15 | 276 MPa | 503 MPa | 324 MPa | 13 ksi | 193 MPa | 74 ksi | 29 MPa | > 85 MPa | 140 MPa | > 400 MPa | 276 MPa | 276 MPa | > 50 ksi | 70 MPa | 350 MPa | 50 MPa | > 110 MPa | 55 MPa | no data | no data | > 125 MPa | > 80 MPa | 350 MPa | 21 ksi | > 255 MPa | 28000 psi | > 414 MPa | no data | no data | no data |
| Tensile strength, O (annealed) temper | 160 to 200 MPa16 | 310 MPa | 572 MPa | 469 MPa | 28 ksi | 228 MPa | 80 ksi | 88 MPa | 105 to 145 MPa | 300 MPa | > 460 MPa | 427 MPa | 427 MPa | > 62 ksi | 160 MPa | 420 MPa | 110 MPa | > 140 MPa | 124 MPa | 270 to 350 MPa | 300 MPa | 275 to 350 MPa | 190 to 260 MPa | 410 MPa | 27 ksi | > 300 MPa | 32000 psi | > 483 MPa | 180 to 195 MPa | no data | no data |
| Elongation A minimum, H22/H32 temper (range by thickness) | 4 to 12 %17 | 17 % | 11 % | 19 % | 25 % | 12 % | 8 % | 50 to 65 % | 4 to 8 % | 16 % | > 6 % | 18 % | 18 % | > 6 % | 12 % | > 5 % | 25 % | > 8 % | 12 % | > 2 % | 20 % | > 12 % | > 12 % | 4 % | 8 % | > 9 % | > 8 % | > 7 % | > 1 % | no data | no data |
| Elongation A minimum, O/H111 temper (range by thickness) | 13 to 18 %18 | 17 % | 11 % | 19 % | 25 % | 12 % | 8 % | 50 to 65 % | 4 to 8 % | 16 % | > 6 % | 18 % | 18 % | > 6 % | 12 % | > 5 % | 25 % | > 8 % | 12 % | > 2 % | 20 % | > 12 % | > 12 % | 4 % | 8 % | > 9 % | > 8 % | > 7 % | > 1 % | no data | no data |
| Yield strength Rp0.2 minimum, H34 temper (AS/NZS 1734) | > 180 MPa19 | 276 MPa | 503 MPa | 324 MPa | 13 ksi | 193 MPa | 74 ksi | 29 MPa | > 85 MPa | 140 MPa | > 400 MPa | 276 MPa | 276 MPa | > 50 ksi | 70 MPa | 350 MPa | 50 MPa | > 110 MPa | 55 MPa | no data | no data | > 125 MPa | > 80 MPa | 350 MPa | 21 ksi | > 255 MPa | 28000 psi | > 414 MPa | no data | no data | no data |
| Tensile strength, H34 temper (AS/NZS 1734) | 235 to 285 MPa20 | 310 MPa | 572 MPa | 469 MPa | 28 ksi | 228 MPa | 80 ksi | 88 MPa | 105 to 145 MPa | 300 MPa | > 460 MPa | 427 MPa | 427 MPa | > 62 ksi | 160 MPa | 420 MPa | 110 MPa | > 140 MPa | 124 MPa | 270 to 350 MPa | 300 MPa | 275 to 350 MPa | 190 to 260 MPa | 410 MPa | 27 ksi | > 300 MPa | 32000 psi | > 483 MPa | 180 to 195 MPa | no data | no data |
Why choose it, and why not
Good for
- Marine and sheet-metal structures, where seawater and atmospheric corrosion resistance matter (Aalco, Atlas).
- Formed and welded sheet: H22 and H24 are readily weldable (Aalco) and have good formability (Euralliage).
- Anodising for decorative and technical finishes (Smith: very good anodising properties).
Watch out for
- Strength is modest: 120 MPa minimum proof stress in H22.
- Welds lose strength: a good weld reaches up to about 160 MPa (Smith).
- The fuel-tank and satellite uses rest on supplier claims; no spacecraft qualification standard for 5251 was found in this run.
- The two SDS family sheets disagree on the solid's hazard status, and neither is specific to 5251.
- Datasheets quote different standards (BS EN 485-2 and AS/NZS 1734), so the limits are not interchangeable.
Aluminium alloy 5251 is a weldable, corrosion-resistant magnesium alloy for marine and sheet-metal structures, with a minimum H22 proof stress of 120 MPa at 2.69 g/cm3. Its spacecraft uses are one supplier's claim, and the profile has no spacecraft qualification, outgassing, atomic-oxygen or radiation data.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Other names and standards
The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.
| System | Codes |
|---|---|
| UNS | A95251 |
| EN | 3.3525 |
| EN name | EN AW-5251 |
| DIN | AlMg2Mn0.3 |
| BS | NS4 |
| ISO | AlMg2 |
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Density, alloy 5251 (sheet and plate, H22 datasheet) | Value printed in a stockholder datasheet, Physical Properties section | grade 5251 (AlMg2)temperature not statedform sheet and plate (H22 datasheet) | — |
| 2 | Density, alloy 5251 (typical values) | Typical value printed in a datasheet, Physical Properties (Typical values) table | grade 5251temperature not statedbasis typical values, as printed | — |
| 3 | Melting range (solidus to liquidus), alloy 5251 | Solidus and liquidus printed as separate values in a datasheet | grade 5251pressure not statednote on form solidification temperature and melting temperature as printed | — |
| 4 | Modulus of elasticity, alloy 5251 | Value printed in a stockholder datasheet, Physical Properties section | grade 5251temperature not stated | — |
| 5 | Thermal conductivity at 25 °C, alloy 5251 (typical values) | — | grade 5251temperature 25 °Cbasis typical values, as printed | Smith prints 149 W/m.K and Euralliage prints 149 W m-1 K-1 with no temperature, and Aalco prints 134 W/m.K with no temperature. The datasheets do not agree, so the rows are kept separate. |
| 6 | Thermal conductivity, alloy 5251 (Smith typical values) | Typical value printed in a datasheet, Typical Mechanical Properties table | grade 5251temperature not statedbasis typical values, as printed | — |
| 7 | Mean coefficient of thermal expansion, 20 to 100 °C, alloy 5251 | — | grade 5251temperature range 20 to 100 °Cbasis typical values, as printed | — |
| 8 | Specific heat capacity, alloy 5251 | Value printed in a datasheet, Table 2 physical and elastic properties | grade 5251temperature not statedunit in source J kg⁻¹ K⁻¹ | — |
| 9 | Electrical resistivity, alloy 5251 (typical values) | — | grade 5251temperature not statedbasis typical values, as printed | — |
| 10 | Electrical conductivity, alloy 5251 (% IACS) | Value printed in a datasheet, Typical Mechanical Properties table | grade 5251temperature not stated | Electrical conductivity is not a canonical property name, so it is entered under its own name. Euralliage prints 37.5 %IACS, which is not entered as a separate row. |
| 11 | Yield strength Rp0.2 minimum, H22 temper | Minimum value printed in a stockholder datasheet that quotes the standard | grade 5251temper H22thickness 0.2 to 25 mmstandard BS EN 485-2:2008measure proof stress, minimumproduct form sheet and plate | — |
| 12 | Tensile strength, H22 temper | Range printed in a stockholder datasheet that quotes the standard | grade 5251temper H22thickness 0.2 to 25 mmstandard BS EN 485-2:2008product form sheet and plate | — |
| 13 | Yield strength Rp0.2 minimum, H24 temper | Minimum value printed in a stockholder datasheet that quotes the standard | grade 5251temper H24thickness 0.2 to 12.5 mmstandard BS EN 485-2:2008measure proof stress, minimumproduct form sheet and plate | — |
| 14 | Tensile strength, H24 temper | Range printed in a stockholder datasheet that quotes the standard | grade 5251temper H24thickness 0.2 to 12.5 mmstandard BS EN 485-2:2008product form sheet and plate | — |
| 15 | Yield strength Rp0.2 minimum, O (annealed) temper | Minimum value printed in an online article that tabulates BS EN 485-2 values by temper | grade 5251temper O (soft)thickness 0.2 to 50 mmstandard BS EN 485-2:2008measure proof stress, minimumproduct form sheet and plate | — |
| 16 | Tensile strength, O (annealed) temper | Range printed in an online article that tabulates BS EN 485-2 values by temper | grade 5251temper O (soft)thickness 0.2 to 50 mmstandard BS EN 485-2:2008product form sheet and plate | — |
| 17 | Elongation A minimum, H22/H32 temper (range by thickness) | Minimum elongation printed as a range by thickness in a datasheet | grade 5251temper H22/H32thickness 0.2 to 25.0 mmstandard EN 485-2 (as printed in table) | — |
| 18 | Elongation A minimum, O/H111 temper (range by thickness) | Minimum elongation printed as a range by thickness in a datasheet | grade 5251temper O/H111thickness 0.2 to 12.5 mmstandard EN 485-2 (as printed in table) | — |
| 19 | Yield strength Rp0.2 minimum, H34 temper (AS/NZS 1734) | Minimum value printed in a datasheet that quotes the Australian and New Zealand standard | grade 5251temper H34standard AS/NZS 1734 (Australia and New Zealand flat-rolled specification)measure 0.2% proof, minimumproduct form flat rolled product | This is an Australia and New Zealand specification, not BS EN 485-2, so its limits are not interchangeable with the H22 and H24 rows above. |
| 20 | Tensile strength, H34 temper (AS/NZS 1734) | Range printed in a datasheet that quotes the Australian and New Zealand standard | grade 5251temper H34standard AS/NZS 1734product form flat rolled product | — |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Marine atmosphere and seawater spray | low | 5251 is described as highly corrosion resistant in marine environments.1 |
| Stress corrosion cracking | low | Low magnesium content keeps 5251 out of the stress corrosion cracking range of higher-magnesium alloys.2 |
| Industrial, sea and country atmospheres | low | Euralliage rates the corrosion indices for 5251 as very good in sea, industrial and country atmospheres.3 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Marine atmosphere and seawater spray | Aalco says it has high corrosion resistance particularly in marine environments. Smith says it can be used in normal, industrial and marine environments without problems and is particularly suited to offshore applications. Atlas says it is acceptable in many marine environments. | basis datasheet statements; no exposure time, site or test data printed |
| 2 | Stress corrosion cracking | Atlas says the magnesium content is low enough that 5251 does not suffer from the stress corrosion cracking that can affect alloys with more than about 3.5 % Mg, such as 5083. | basis statement in datasheet; no test data printedthreshold in source more than about 3½ % Mg |
| 3 | Industrial, sea and country atmospheres | Euralliage gives Very good for general corrosion, industrial, sea and country atmosphere corrosion, stress corrosion, exfoliation and intercrystalline corrosion. The page gives ratings only, with no rates or durations. | basis qualitative index ratings for information only; no exposure time printed |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
The solid alloy is described as not hazardous in one sheet, but processing dust and welding fume are the real concern.
- Solid sheet
- The Texarkana 5xxx-series sheet says the formed solid as shipped is not hazardous. The Kaiser sheet says the material is considered hazardous under US hazard communication rules, so the two family sheets disagree on the solid's status.
- Dust and fumes
- Kaiser says dust may irritate the eyes, skin and airways, and Texarkana notes combustible dust concentrations during processing. Welding and cutting may release hazardous fumes.
If it fails
The failure routes in the sources are weld strength loss and softening by heat. No spacecraft service data for 5251 was found.
- Weld zone
- Smith says a good weld is likely to have strength of up to 160 MPa maximum, against a minimum tensile strength of 190 MPa for H22 sheet (Aalco).
- Heat
- Atlas says heating cold-worked sheet to about 345 °C softens it, so the cold-work strength is removed.
Handling and storage
- Pick the temper
- The datasheets quote the temper by thickness. H22 has a minimum proof stress of 120 MPa, H24 of 140 MPa and O of 60 MPa.
- Filler
- Aalco recommends 5356 filler for welding 5251 to itself and to most other 5XXX and 6XXX alloys.
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Strength loss in welds of strain-hardened tempersmoderate severity | Welding H22 or H24 sheet, with filler 5356 (Aalco) or 5056A or 5154A (Smith)Smith says a good weld is likely to have strength of up to 160 MPa maximum, depending on the welding type and quality. Atlas says welding strain-hardened tempers reduces strength in the heat-affected zone. |
| Softening by heating cold-worked sheetlow severity | Heating cold-worked material to about 345 °CAtlas says 5251 can be annealed by heating to 345 °C, holding until the temperature is uniform, then cooling. The cold-work strength is lost. No hold time or property data after heating is printed. |
| Age softening after cold worklow severity | Standing at room temperature after cold work, before stabilisationAtlas says the alloy spontaneously age-softens right after cold work until it reaches a stable condition. Mill products are supplied with stable properties, so the effect applies to unstabilised cold-worked stock. |
Handling and storage
- Aalco rates brazability as poor. It recommends filler 5356 for welding 5251 to itself and to 6XXX, 7XXX and most other 5XXX alloys, and 4043 for welding to 5005, 5020, 1XXX or 3XXX alloys.
- Atlas says machinability of the softer O and H32 tempers is poor, and that harder tempers such as H34 are somewhat easier to machine.
- Prevent dust accumulation to minimise explosion hazard, and avoid generating dust (Texarkana SDS).
Supply and geography
How common the raw materials are and where they come from.
Primary aluminium smelter production (world, 2025 estimated)
- Top producers (2025)
- China 60.8%, India 5.7%, Russia 5.3%, Canada 4.5%
- Recycling
- USGS: in 2025 aluminium recovered from purchased scrap in the United States was about 3.6 million tons, 56 % from new scrap and 44 % from old scrap. Recovery from old scrap was equivalent to about 28 % of apparent consumption.
- Substitutes
- USGS: composites can substitute for aluminium in aircraft fuselages and wings. Magnesium, steel and titanium can substitute in ground transportation uses. Copper can replace aluminium in electrical and heat-exchange applications.
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: aluminium-5251
spore_version: 0.2
family: aluminium-alloys
name: Aluminium alloy 5251
abbreviation: AlMg2
role: marine and sheet-metal structural alloy
category: metals
type: aluminium
summary: |
Aluminium alloy 5251 (EN AW-5251, AlMg2Mn0.3) is a non-heat-treatable wrought aluminium-magnesium alloy with 1.70 to 2.40 wt% magnesium. Its density is 2.69 g/cm3 in the Aalco H22 datasheet. Cold work sets the H tempers: H22 has a minimum proof stress of 120 MPa and a tensile strength of 190 to 230 MPa, and H24 has 140 MPa and 210 to 250 MPa. Datasheets rate its corrosion resistance in marine air highly and call it readily weldable. Suppliers list it for boats, panelling and aircraft fuel tanks, and one supplier claims use in satellite shells.
best_for: Welded marine and sheet-metal structures where seawater corrosion resistance and weldability matter more than peak strength, at 2.69 g/cm3
weakest_at: 'Strength compared with heat-treatable alloys: H22 minimum proof stress is 120 MPa, and a good weld reaches only about 160 MPa (Smith)'
identity:
formula: AlMg2Mn0.3 (aluminium with 1.70 to 2.40 wt% Mg, 0.10 to 0.50 wt% Mn, up to 0.50 wt% Fe, up to 0.40 wt% Si, balance Al; limits as printed to BS EN 573-3 in the Aalco H22 datasheet)
source: aalco-5251-h22
where: Chemical composition table (BS EN573-3:2009), rows Magnesium, Manganese, Iron and Silicon. The AlMg2Mn0.3 name is printed on the Modulus Metal page under the DIN 1725-1 entry.
designations:
- system: UNS
code: A95251
source: modulus-5251
where: Designation table, UNS number row
- system: EN
code: '3.3525'
source: modulus-5251
where: Designation table, EN number row
- system: EN name
code: EN AW-5251
source: modulus-5251
where: Designation table, EN name row (EN AW-5251 (EN AW-Al Mg2))
- system: DIN
code: AlMg2Mn0.3
source: modulus-5251
where: Other designations list, Germany line (3.3525/AlMg2Mn0.3 to DIN 1725-1)
- system: ISO
code: AlMg2
source: modulus-5251
where: Other designations list, International line (AlMg2 to ISO 209-1)
- system: BS
code: NS4
note: former British Standard designation; Smith says the previous BS specification was known as NS4 H3
source: smith-5251
where: Title line 5251 (NS4) and Technical Description
tags:
environments: []
stresses: []
applications:
- structures
- propulsion-and-tanks
- thermal-control
properties:
- benchmark: density
label: Density, alloy 5251 (sheet and plate, H22 datasheet)
value: 2.69
unit: g/cm3
scope: material
conditions:
grade: 5251 (AlMg2)
temperature: not stated
form: sheet and plate (H22 datasheet)
method: Value printed in a stockholder datasheet, Physical Properties section
status: ground
source: aalco-5251-h22
where: Physical Properties table, row Density
- benchmark: density
label: Density, alloy 5251 (typical values)
value: 2680
unit: kg/m3
scope: material
conditions:
grade: '5251'
temperature: not stated
basis: typical values, as printed
method: Typical value printed in a datasheet, Physical Properties (Typical values) table
status: ground
source: atlas-5251
where: Physical Properties (Typical values) table, column Density (kg/m3), row 5251
- benchmark: melting_point
label: Melting range (solidus to liquidus), alloy 5251
value: 605
value_high: 650
bound: range
unit: °C
scope: material
conditions:
grade: '5251'
pressure: not stated
note_on_form: solidification temperature and melting temperature as printed
method: Solidus and liquidus printed as separate values in a datasheet
status: ground
source: euralliage-5251
where: Table 2, Solidification temperature T_sol 605 and Melting temperature T_liq 650
- benchmark: elastic_modulus
label: Modulus of elasticity, alloy 5251
value: 70
unit: GPa
scope: material
conditions:
grade: '5251'
temperature: not stated
method: Value printed in a stockholder datasheet, Physical Properties section
status: ground
source: aalco-5251-h22
where: Physical Properties table, row Modulus of Elasticity
- benchmark: thermal_conductivity
label: Thermal conductivity at 25 °C, alloy 5251 (typical values)
value: 138
unit: W/(m·K)
scope: material
conditions:
grade: '5251'
temperature: 25 °C
basis: typical values, as printed
method: Typical value printed in a datasheet
status: ground
note: Smith prints 149 W/m.K and Euralliage prints 149 W m-1 K-1 with no temperature, and Aalco prints 134 W/m.K with no temperature. The datasheets do not agree, so the rows are kept separate.
source: atlas-5251
where: Physical Properties (Typical values) table, column Thermal Conductivity at 25 °C
- benchmark: thermal_conductivity
label: Thermal conductivity, alloy 5251 (Smith typical values)
value: 149
unit: W/(m·K)
scope: material
conditions:
grade: '5251'
temperature: not stated
basis: typical values, as printed
method: Typical value printed in a datasheet, Typical Mechanical Properties table
status: ground
source: smith-5251
where: Typical Mechanical Properties table, row Thermal conductivity W/m.K
- benchmark: cte
label: Mean coefficient of thermal expansion, 20 to 100 °C, alloy 5251
value: 23.8
unit: µm/m/°C
scope: material
conditions:
grade: '5251'
temperature_range: 20 to 100 °C
basis: typical values, as printed
method: Typical value printed in a datasheet
status: ground
source: atlas-5251
where: Physical Properties (Typical values) table, column Mean Coefficient of Thermal Expansion 20-100°C
- benchmark: specific_heat
label: Specific heat capacity, alloy 5251
value: 898
unit: J/(kg·K)
scope: material
conditions:
grade: '5251'
temperature: not stated
unit_in_source: J kg⁻¹ K⁻¹
method: Value printed in a datasheet, Table 2 physical and elastic properties
status: ground
source: euralliage-5251
where: Table 2, row Specific heat C_p
- benchmark: electrical_resistivity
label: Electrical resistivity, alloy 5251 (typical values)
value: 50
unit: nΩ·m
scope: material
conditions:
grade: '5251'
temperature: not stated
basis: typical values, as printed
method: Typical value printed in a datasheet
status: ground
source: atlas-5251
where: Physical Properties (Typical values) table, column Electrical Resistivity (nΩ.m)
- benchmark: electrical_conductivity
label: Electrical conductivity, alloy 5251 (% IACS)
value: 39.4
unit: '% IACS'
scope: material
conditions:
grade: '5251'
temperature: not stated
method: Value printed in a datasheet, Typical Mechanical Properties table
status: ground
note: Electrical conductivity is not a canonical property name, so it is entered under its own name. Euralliage prints 37.5 %IACS, which is not entered as a separate row.
source: smith-5251
where: Typical Mechanical Properties table, row Electrical conductivity % IACS
- benchmark: yield_strength
label: Yield strength Rp0.2 minimum, H22 temper
value: 120
bound: lower
unit: MPa
scope: material
conditions:
grade: '5251'
temper: H22
thickness: 0.2 to 25 mm
standard: BS EN 485-2:2008
measure: proof stress, minimum
product_form: sheet and plate
method: Minimum value printed in a stockholder datasheet that quotes the standard
status: ground
source: aalco-5251-h22
where: Mechanical Properties table, row H22, column Proof Stress
- benchmark: ultimate_tensile_strength
label: Tensile strength, H22 temper
value: 190
value_high: 230
bound: range
unit: MPa
scope: material
conditions:
grade: '5251'
temper: H22
thickness: 0.2 to 25 mm
standard: BS EN 485-2:2008
product_form: sheet and plate
method: Range printed in a stockholder datasheet that quotes the standard
status: ground
source: aalco-5251-h22
where: Mechanical Properties table, row H22, column Tensile Strength
- benchmark: yield_strength
label: Yield strength Rp0.2 minimum, H24 temper
value: 140
bound: lower
unit: MPa
scope: material
conditions:
grade: '5251'
temper: H24
thickness: 0.2 to 12.5 mm
standard: BS EN 485-2:2008
measure: proof stress, minimum
product_form: sheet and plate
method: Minimum value printed in a stockholder datasheet that quotes the standard
status: ground
source: aalco-5251-h24
where: Mechanical Properties table, row H24, column Proof Stress
- benchmark: ultimate_tensile_strength
label: Tensile strength, H24 temper
value: 210
value_high: 250
bound: range
unit: MPa
scope: material
conditions:
grade: '5251'
temper: H24
thickness: 0.2 to 12.5 mm
standard: BS EN 485-2:2008
product_form: sheet and plate
method: Range printed in a stockholder datasheet that quotes the standard
status: ground
source: aalco-5251-h24
where: Mechanical Properties table, row H24, column Tensile Strength
- benchmark: yield_strength
label: Yield strength Rp0.2 minimum, O (annealed) temper
value: 60
bound: lower
unit: MPa
scope: material
conditions:
grade: '5251'
temper: O (soft)
thickness: 0.2 to 50 mm
standard: BS EN 485-2:2008
measure: proof stress, minimum
product_form: sheet and plate
method: Minimum value printed in an online article that tabulates BS EN 485-2 values by temper
status: ground
source: azom-5251
where: Mechanical Properties by Temper table, row O (soft), column Proof Stress
- benchmark: ultimate_tensile_strength
label: Tensile strength, O (annealed) temper
value: 160
value_high: 200
bound: range
unit: MPa
scope: material
conditions:
grade: '5251'
temper: O (soft)
thickness: 0.2 to 50 mm
standard: BS EN 485-2:2008
product_form: sheet and plate
method: Range printed in an online article that tabulates BS EN 485-2 values by temper
status: ground
source: azom-5251
where: Mechanical Properties by Temper table, row O (soft), column Tensile Strength
- benchmark: elongation
label: Elongation A minimum, H22/H32 temper (range by thickness)
value: 4
value_high: 12
bound: range
unit: '%'
scope: material
conditions:
grade: '5251'
temper: H22/H32
thickness: 0.2 to 25.0 mm
standard: EN 485-2 (as printed in table)
method: Minimum elongation printed as a range by thickness in a datasheet
status: ground
source: euralliage-5251
where: Table 3, Sheets (EN 485-2), row H22/H32, column A % min
- benchmark: elongation
label: Elongation A minimum, O/H111 temper (range by thickness)
value: 13
value_high: 18
bound: range
unit: '%'
scope: material
conditions:
grade: '5251'
temper: O/H111
thickness: 0.2 to 12.5 mm
standard: EN 485-2 (as printed in table)
method: Minimum elongation printed as a range by thickness in a datasheet
status: ground
source: euralliage-5251
where: Table 3, Sheets (EN 485-2), row O/H111, column A % min
- benchmark: yield_strength
label: Yield strength Rp0.2 minimum, H34 temper (AS/NZS 1734)
value: 180
bound: lower
unit: MPa
scope: material
conditions:
grade: '5251'
temper: H34
standard: AS/NZS 1734 (Australia and New Zealand flat-rolled specification)
measure: 0.2% proof, minimum
product_form: flat rolled product
method: Minimum value printed in a datasheet that quotes the Australian and New Zealand standard
status: ground
note: This is an Australia and New Zealand specification, not BS EN 485-2, so its limits are not interchangeable with the H22 and H24 rows above.
source: atlas-5251
where: Mechanical Property Specification table, row 5251-H34, column Yield Strength 0.2% Proof (MPa) min.
- benchmark: ultimate_tensile_strength
label: Tensile strength, H34 temper (AS/NZS 1734)
value: 235
value_high: 285
bound: range
unit: MPa
scope: material
conditions:
grade: '5251'
temper: H34
standard: AS/NZS 1734
product_form: flat rolled product
method: Range printed in a datasheet that quotes the Australian and New Zealand standard
status: ground
source: atlas-5251
where: Mechanical Property Specification table, row 5251-H34, column Tensile Strength (MPa)
corrosion:
- environment: Marine atmosphere and seawater spray
headline: 5251 is described as highly corrosion resistant in marine environments.
effect: Aalco says it has high corrosion resistance particularly in marine environments. Smith says it can be used in normal, industrial and marine environments without problems and is particularly suited to offshore applications. Atlas says it is acceptable in many marine environments.
rating: low
conditions:
basis: datasheet statements; no exposure time, site or test data printed
source: aalco-5251-h22
where: Description paragraph (high corrosion resistance particularly in marine environments)
- environment: Stress corrosion cracking
headline: Low magnesium content keeps 5251 out of the stress corrosion cracking range of higher-magnesium alloys.
effect: Atlas says the magnesium content is low enough that 5251 does not suffer from the stress corrosion cracking that can affect alloys with more than about 3.5 % Mg, such as 5083.
rating: low
conditions:
basis: statement in datasheet; no test data printed
threshold_in_source: more than about 3½ % Mg
source: atlas-5251
where: Corrosion Resistance section, first paragraph
- environment: Industrial, sea and country atmospheres
headline: Euralliage rates the corrosion indices for 5251 as very good in sea, industrial and country atmospheres.
effect: Euralliage gives Very good for general corrosion, industrial, sea and country atmosphere corrosion, stress corrosion, exfoliation and intercrystalline corrosion. The page gives ratings only, with no rates or durations.
rating: low
conditions:
basis: qualitative index ratings for information only; no exposure time printed
source: euralliage-5251
where: Corrosion (properties, for information only) list
risks:
hazards:
- text: 'Kaiser Aluminum SDS for aluminium and its alloys (a generic sheet, not 5251-specific): the product is solid metallic pieces and may form explosive dust/air mixtures if high concentrations of dust are suspended in air. Dust or fumes may irritate the eyes, skin and respiratory tract. The same sheet says the material is considered hazardous under 29 CFR 1910.1200, which conflicts with the Texarkana sheet below.'
ghs: []
source: kaiser-al-sds
where: Section 2 Hazards Identification; Fire and explosion hazards; Component Information
- text: 'Texarkana Aluminum SDS for 5xxx-series alloys (a family sheet, not 5251-specific): the formed solid as shipped is not hazardous, but processing can generate combustible dust. Signal word Warning, with the hazard statement May form combustible dust concentrations in air during processing and handling. Welding, cutting or processing may release hazardous dust or fumes.'
ghs: []
source: tex-5xxx-sds
where: Section 2 Hazards Identification (signal word and hazard statement); Additional Information; Symptoms and Injuries
failure_risks:
- mode: Strength loss in welds of strain-hardened tempers
trigger: Welding H22 or H24 sheet, with filler 5356 (Aalco) or 5056A or 5154A (Smith)
consequence: Smith says a good weld is likely to have strength of up to 160 MPa maximum, depending on the welding type and quality. Atlas says welding strain-hardened tempers reduces strength in the heat-affected zone.
severity: moderate
source: smith-5251
where: Welding section
- mode: Softening by heating cold-worked sheet
trigger: Heating cold-worked material to about 345 °C
consequence: Atlas says 5251 can be annealed by heating to 345 °C, holding until the temperature is uniform, then cooling. The cold-work strength is lost. No hold time or property data after heating is printed.
severity: low
source: atlas-5251
where: Heat Treatment section
- mode: Age softening after cold work
trigger: Standing at room temperature after cold work, before stabilisation
consequence: Atlas says the alloy spontaneously age-softens right after cold work until it reaches a stable condition. Mill products are supplied with stable properties, so the effect applies to unstabilised cold-worked stock.
severity: low
source: atlas-5251
where: Heat Treatment section, second paragraph
side_effects: []
handling:
- text: Aalco rates brazability as poor. It recommends filler 5356 for welding 5251 to itself and to 6XXX, 7XXX and most other 5XXX alloys, and 4043 for welding to 5005, 5020, 1XXX or 3XXX alloys.
source: aalco-5251-h22
where: Weldability table and filler text
- text: Atlas says machinability of the softer O and H32 tempers is poor, and that harder tempers such as H34 are somewhat easier to machine.
source: atlas-5251
where: Machining section
- text: Prevent dust accumulation to minimise explosion hazard, and avoid generating dust (Texarkana SDS).
source: tex-5xxx-sds
where: Section 2 precautionary statements
mitigations: []
uses:
- application: structures
device: Boats, marine structures, panelling and vehicle panels
example: Aalco lists boats, panelling and pressings, marine structures, aircraft parts, vehicle panels, furniture tubing, silos and containers as typical uses of 5251. Atlas lists small marine craft (tinnies) as typical applications.
source: aalco-5251-h22
where: Typical Uses paragraph; Atlas Typical Applications section
- application: propulsion-and-tanks
device: Aircraft fuel tanks and oxygen cylinders (supplier claim)
example: Chalco says 5251 sheet can be used to manufacture aircraft fuselage shells, fuel tanks and oxygen cylinders. This is a supplier product-page claim, not a qualification standard.
source: chalco-5251-plate
where: Stated applications list on the 5251 O/H16/H26 Aerospace Aluminum Sheet page
- application: structures
device: Satellite shells and missile structures (supplier claim)
example: The same Chalco page says 5251 has also been used on spacecraft components such as satellite shells and missile structures. No spacecraft qualification data for 5251 was opened in this run.
source: chalco-5251-plate
where: Stated applications list, spacecraft sentence
- application: thermal-control
device: Heat transfer devices, pressure vessels and boilers
example: Smith lists heat transfer devices, pressure vessels, boiler making, chemical industry and pharmaceutical work among typical applications for its 5251 sheet.
source: smith-5251
where: Typical Applications list
supply:
- subject: Primary aluminium smelter production (world, 2025 estimated)
producers:
- country: China
share_percent: 60.8
year: 2025
- country: India
share_percent: 5.7
year: 2025
- country: Russia
share_percent: 5.3
year: 2025
- country: Canada
share_percent: 4.5
year: 2025
critical_lists: []
recycling: 'USGS: in 2025 aluminium recovered from purchased scrap in the United States was about 3.6 million tons, 56 % from new scrap and 44 % from old scrap. Recovery from old scrap was equivalent to about 28 % of apparent consumption.'
substitutes:
- 'USGS: composites can substitute for aluminium in aircraft fuselages and wings. Magnesium, steel and titanium can substitute in ground transportation uses. Copper can replace aluminium in electrical and heat-exchange applications.'
source: usgs-mcs2026-aluminum
where: 'Smelter production table, column 2025e: China 45,000, India 4,200, Russia 3,900, Canada 3,300, world total 74,000 thousand t. Shares calculated by Space Mushroom from those printed values, not printed by USGS. Recycling paragraph; Substitutes paragraph.'
documents:
- title: 'Aalco datasheet: Aluminium Alloy 5251 H22 Sheet and Plate (BS EN 573-3, BS EN 485-2)'
type: datasheet
url: https://www.aalco.co.uk/datasheets/Aluminium-Alloy-5251-H22-Sheet-and-Plate_150.ashx
- title: 'Aalco datasheet: Aluminium Alloy 5251 H24 Sheet and Plate'
type: datasheet
url: https://www.aalco.co.uk/datasheets/Aluminium-Alloy-5251-H24-Sheet-and-Plate_151.ashx
- title: 'Modulus Metal: Aluminum 5251 Material Data Sheet'
type: datasheet
url: https://www.modulusmetal.com/aluminum-5251-material-data-sheet/
- title: 'Atlas Steels: Aluminium Alloy 5251 Data Sheet (revised 24/06/2021)'
type: datasheet
url: https://atlassteels.com.au/wp-content/uploads/2021/08/Aluminium-Alloy-5251-Data-Sheet-24-06-21.pdf
year: 2021
- title: 'Smiths Metal Centres: 5251 (NS4) Technical Datasheet'
type: datasheet
url: https://www.smithmetal.com/pdf/aluminium/5xxx/5251.pdf
year: 2023
- title: 'Euralliage: 5251 (AW-AlMg2) product datasheet'
type: datasheet
url: https://www.euralliage.com/5251_english.htm
- title: 'AZoM: Aluminium Alloys, Aluminium 5251 Properties, Fabrication and Applications'
type: database
url: https://www.azom.com/article.aspx?ArticleID=2805
- title: 'USGS Mineral Commodity Summaries 2026: Aluminum'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-aluminum.pdf
year: 2026
- title: 'Chalco: 5251 O/H16/H26 Aerospace Aluminum Sheet (supplier page)'
type: datasheet
url: https://www.chalcoaluminum.com/application/aluminum-aerospace/5251-plate/
- title: Kaiser Aluminum safety data sheet, aluminum and alloys (2017, generic)
type: sds
url: https://www.kaiseraluminum.com/files/msds/2017-Aluminum-and-Alloys.pdf
year: 2017
- title: Texarkana Aluminum safety data sheet, 5xxx series alloys (Rev 5-14-2020, family sheet)
type: sds
url: https://www.texarkanaaluminum.com/PDF/Aluminum%205xxx%20Series%20Alloys%20SDS%20Rev%205-14-2020.pdf
year: 2020
gaps:
- No spacecraft qualification data for 5251 (AMS, ECSS or NASA material specification) was found. The satellite and missile use rests on a single supplier page (Chalco), and the fuel-tank and oxygen-cylinder uses are also supplier claims.
- No NASA outgassing data (total mass loss or collected volatile condensable material), atomic-oxygen erosion yield, radiation effects or cryogenic toughness for 5251 was found or opened.
- Chalco prints fatigue strengths of 55 to 75 MPa for 5251 tempers. These are not entered, because the table gives no test standard, specimen or stress ratio.
- PubChem's GHS record for aluminium was blocked by a verification page, and no 5251-specific SDS was found. The hazard entries rest on two generic or family SDS sheets (Kaiser and Texarkana) that disagree on classification of the solid.
- The USGS aluminum summary read here does not name aluminium on a critical-minerals list, so critical_lists is left empty. The USGS text was read from the 2026 summary; the critical-minerals list itself was not opened.
- 'Brinell hardness (Aalco H22 56 HB, H24 62 HB; AZoM O 44 HB) is not entered: ''hardness'' is not a canonical property name in this site''s property list.'
- Smith's typical tensile range (200 to 240 MPa) and minimum yield (130 MPa, approximate only) are not entered, because Smith does not name the temper for those rows and its values differ from the BS EN 485-2 values for H22.
- Euralliage prints electrical resistivity as 46 nW m, with the ohm sign missing, so that value is not entered. Its electrical conductivity of 37.5 %IACS is also not entered, since Smith's 39.4 %IACS is recorded.
- Poisson's ratio (0.33, Euralliage) and shear strength (125 N/mm2, Smith) were read but are not entered. Neither is in the property canon as a Smith-supported row for this grade.
- The AA (Aluminum Association) designation 5251 appears on the Modulus Metal page, but this site does not have an AA system code, so it is not entered. Atlas says 5251 is not in ASTM B209M, so no ASTM code is listed.
- The casting and rolling route, and the melting practice, are not described in any source opened in this run.
sources:
aalco-5251-h22:
title: Aluminium Alloy 5251 H22 Sheet and Plate (Aalco commercial alloy datasheet)
url: https://www.aalco.co.uk/datasheets/Aluminium-Alloy-5251-H22-Sheet-and-Plate_150.ashx
kind: datasheet
license: Stockholder datasheet (cited, not reproduced)
aalco-5251-h24:
title: Aluminium Alloy 5251 H24 Sheet and Plate (Aalco commercial alloy datasheet)
url: https://www.aalco.co.uk/datasheets/Aluminium-Alloy-5251-H24-Sheet-and-Plate_151.ashx
kind: datasheet
license: Stockholder datasheet (cited, not reproduced)
modulus-5251:
title: Aluminum 5251 Material Data Sheet (Modulus Metal)
url: https://www.modulusmetal.com/aluminum-5251-material-data-sheet/
kind: datasheet
license: Supplier web page (cited, not reproduced)
atlas-5251:
title: Aluminium Alloy 5251 Data Sheet (Atlas Steels, revised 24/06/2021)
url: https://atlassteels.com.au/wp-content/uploads/2021/08/Aluminium-Alloy-5251-Data-Sheet-24-06-21.pdf
year: 2021
kind: datasheet
license: Supplier data sheet (cited, not reproduced)
smith-5251:
title: 5251 (NS4) Technical Datasheet (Smiths Metal Centres)
url: https://www.smithmetal.com/pdf/aluminium/5xxx/5251.pdf
year: 2023
kind: datasheet
license: Supplier data sheet (cited, not reproduced)
euralliage-5251:
title: 5251 (AW-AlMg2) product datasheet (Euralliage)
url: https://www.euralliage.com/5251_english.htm
kind: datasheet
license: Supplier web page (cited, not reproduced)
azom-5251:
title: 'Aluminium Alloys: Aluminium 5251 Properties, Fabrication and Applications (AZoM)'
url: https://www.azom.com/article.aspx?ArticleID=2805
kind: web
license: Web article (cited, not reproduced)
usgs-mcs2026-aluminum:
title: 'Mineral Commodity Summaries 2026: Aluminum (USGS)'
id: USGS MCS 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-aluminum.pdf
year: 2026
kind: report
license: public domain (USGS)
chalco-5251-plate:
title: 5251 O/H16/H26 Aerospace Aluminum Sheet (Chalco supplier page)
url: https://www.chalcoaluminum.com/application/aluminum-aerospace/5251-plate/
kind: web
license: Supplier web page (cited, not reproduced)
kaiser-al-sds:
title: 'Safety Data Sheet: Aluminum and Alloys (Kaiser Aluminum, generic, 2017)'
url: https://www.kaiseraluminum.com/files/msds/2017-Aluminum-and-Alloys.pdf
year: 2017
kind: datasheet
license: Manufacturer safety data sheet (cited, not reproduced)
tex-5xxx-sds:
title: 'Safety Data Sheet: Aluminum 5xxx Series Alloys (Texarkana Aluminum, Rev 5-14-2020, family sheet)'
url: https://www.texarkanaaluminum.com/PDF/Aluminum%205xxx%20Series%20Alloys%20SDS%20Rev%205-14-2020.pdf
year: 2020
kind: datasheet
license: Manufacturer safety data sheet (cited, not reproduced)
license: CC-BY-4.0
updated: '2026-10-26'
review:
status: draft
method: assistant
checked_values: 20
unreachable: 3
caveats: 6
note: 'Values were read by an AI assistant on 2026-10-26 from the pages and PDFs named in each entry. Unreachable: the MakeItFrom 5251 page (403), the PubChem aluminium record (verification page), and the Smith and Kaiser PDFs were read as text with pdftotext. Caveats: the H22 and H24 strength values are BS EN 485-2 minima from one stockholder; the H34 values are an Australian and New Zealand specification; the thermal conductivity differs between datasheets (134, 138 and 149 W/(m·K)); the space uses are one supplier''s claim; the hazard entries rest on two sheets that are not 5251-specific.'
story:
risk_groups:
- title: For people
lead: The solid alloy is described as not hazardous in one sheet, but processing dust and welding fume are the real concern.
level: 1
verdict: Low as solid sheet, higher for dust and fume
points:
- label: Solid sheet
line: The Texarkana 5xxx-series sheet says the formed solid as shipped is not hazardous. The Kaiser sheet says the material is considered hazardous under US hazard communication rules, so the two family sheets disagree on the solid's status.
- label: Dust and fumes
line: Kaiser says dust may irritate the eyes, skin and airways, and Texarkana notes combustible dust concentrations during processing. Welding and cutting may release hazardous fumes.
- title: If it fails
lead: The failure routes in the sources are weld strength loss and softening by heat. No spacecraft service data for 5251 was found.
points:
- label: Weld zone
line: Smith says a good weld is likely to have strength of up to 160 MPa maximum, against a minimum tensile strength of 190 MPa for H22 sheet (Aalco).
- label: Heat
line: Atlas says heating cold-worked sheet to about 345 °C softens it, so the cold-work strength is removed.
- title: Handling and storage
points:
- label: Pick the temper
line: The datasheets quote the temper by thickness. H22 has a minimum proof stress of 120 MPa, H24 of 140 MPa and O of 60 MPa.
- label: Filler
line: Aalco recommends 5356 filler for welding 5251 to itself and to most other 5XXX and 6XXX alloys.
why: Aluminium alloy 5251 is chosen for sheet work that has to bend and weld and resist seawater, with more strength than pure aluminium. Its magnesium content is low enough that Atlas says it avoids the stress corrosion cracking of alloys with more than about 3.5 % Mg. At 2.69 g/cm3 (Aalco H22) it is light compared with steel. Suppliers list it for boats, panelling, pressure work, fuel tanks and, in one supplier's claim, satellite shells.
uses:
- where: Marine and sheet metal work
line: Aalco lists boats, panelling and pressings, marine structures, vehicle panels and containers as typical uses.
- where: Aircraft and spacecraft parts (supplier claims)
line: Chalco says 5251 can be used for aircraft fuselage shells, fuel tanks and oxygen cylinders, and that it has been used for satellite shells and missile structures. These are supplier claims, and no qualification data was opened.
- where: Heat transfer and pressure work
line: Smith lists heat transfer devices, pressure vessels, boiler making and chemical industry work among typical uses of its 5251 sheet.
can_do:
- label: Carry heat
value: 138 W/(m·K)
benchmark: thermal_conductivity
line: Atlas gives 138 W/(m·K) at 25 °C as a typical value. Smith prints 149 and Aalco prints 134, both without a stated temperature, so the datasheets differ.
- label: Strength when soft
value: 60 MPa proof stress (O)
benchmark: yield_strength
line: The O temper has a minimum proof stress of 60 MPa and a tensile strength of 160 to 200 MPa, per the BS EN 485-2 values in the AZoM table.
- label: Strength after cold work
value: 120 MPa proof stress (H22)
benchmark: yield_strength
line: H22 has a minimum proof stress of 120 MPa and a tensile strength of 190 to 230 MPa. H24 has 140 MPa and 210 to 250 MPa.
- label: Weight
value: 2.69 g/cm3
benchmark: density
line: Density is 2.69 g/cm3 in the Aalco datasheet. Atlas gives 2680 kg/m3 as a typical value.
- label: Melting
value: 605 to 650 °C
benchmark: melting_point
line: Euralliage gives a solidus of 605 °C and a liquidus of 650 °C.
- label: Expansion
value: 23.8 µm/m/°C
benchmark: cte
line: Atlas gives a mean thermal expansion of 23.8 µm/m/°C between 20 and 100 °C.
compare: Atlas says the specified yield strength of this alloy in the H32 and H34 tempers is substantially lower than that of its sister alloy in the same tempers, so substitution needs care. The USGS says copper can replace aluminium in electrical and heat-exchange applications, so the two metals compete in conductors and heat exchangers.
compare_rows:
- label: Density
benchmark: density
- label: Thermal conductivity
benchmark: thermal_conductivity
- label: Thermal expansion
benchmark: cte
handling:
- Specify the temper and thickness, because the minimum strengths change with both.
- Weld with 5356 filler, and plan for weld strength of up to about 160 MPa (Smith).
- Control dust during cutting, grinding and welding (Texarkana).
good_for:
- Marine and sheet-metal structures, where seawater and atmospheric corrosion resistance matter (Aalco, Atlas).
- 'Formed and welded sheet: H22 and H24 are readily weldable (Aalco) and have good formability (Euralliage).'
- 'Anodising for decorative and technical finishes (Smith: very good anodising properties).'
watch_out:
- 'Strength is modest: 120 MPa minimum proof stress in H22.'
- 'Welds lose strength: a good weld reaches up to about 160 MPa (Smith).'
- The fuel-tank and satellite uses rest on supplier claims; no spacecraft qualification standard for 5251 was found in this run.
- The two SDS family sheets disagree on the solid's hazard status, and neither is specific to 5251.
- Datasheets quote different standards (BS EN 485-2 and AS/NZS 1734), so the limits are not interchangeable.
verdict: Aluminium alloy 5251 is a weldable, corrosion-resistant magnesium alloy for marine and sheet-metal structures, with a minimum H22 proof stress of 120 MPa at 2.69 g/cm3. Its spacecraft uses are one supplier's claim, and the profile has no spacecraft qualification, outgassing, atomic-oxygen or radiation data.
recipe:
line: Wrought aluminium alloy AlMg2Mn0.3, with magnesium as the main alloying element and manganese as the second (Atlas describes it as a 2 % magnesium, 0.3 % manganese alloy). It is not heat-treatable; strength comes from cold rolling into the H tempers and partial annealing (Atlas). Composition limits are from Aalco (BS EN 573-3). The datasheets do not describe the casting route.
parts:
- name: Aluminium
symbol: Al
share: balance
role: Matrix metal. Aalco prints aluminium as the balance of the composition.
- name: Magnesium
symbol: Mg
share: 1.70 to 2.40 wt%
role: Main alloying element; the alloy is non-heat-treatable and its strength comes from cold work (Atlas).
- name: Manganese
symbol: Mn
share: 0.10 to 0.50 wt%
role: Alloying element, printed with magnesium in the designation AlMg2Mn0.3 (Modulus Metal, DIN 1725-1).
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.
| # | Source | Type | Year | Used for |
|---|---|---|---|---|
| Aluminium Alloy 5251 H22 Sheet and Plate (Aalco commercial alloy datasheet) | datasheet | 8 values | ||
| Aluminium Alloy 5251 H24 Sheet and Plate (Aalco commercial alloy datasheet) | datasheet | 2 values | ||
| Aluminum 5251 Material Data Sheet (Modulus Metal) | datasheet | 0 values | ||
| Aluminium Alloy 5251 Data Sheet (Atlas Steels, revised 24/06/2021) | datasheet | 2021 | 10 values | |
| 5251 (NS4) Technical Datasheet (Smiths Metal Centres) | datasheet | 2023 | 4 values | |
| 5251 (AW-AlMg2) product datasheet (Euralliage) | datasheet | 5 values | ||
| Aluminium Alloys: Aluminium 5251 Properties, Fabrication and Applications (AZoM) | web | 2 values | ||
| Mineral Commodity Summaries 2026: Aluminum (USGS) | report | 2026 | 1 value | |
| 5251 O/H16/H26 Aerospace Aluminum Sheet (Chalco supplier page) | web | 2 values | ||
| Safety Data Sheet: Aluminum and Alloys (Kaiser Aluminum, generic, 2017) | datasheet | 2017 | 1 value | |
| Safety Data Sheet: Aluminum 5xxx Series Alloys (Texarkana Aluminum, Rev 5-14-2020, family sheet) | datasheet | 2020 | 2 values |