Aluminium alloy 5083 5083
Al-Mg alloy
Also known as UNS A95083, EN 3.3547, EN name EN AW-5083, EN name AlMg4.5Mn0.7, AA 5083, AMS 4056 · 1 more
5083 is a wrought aluminium-magnesium alloy with 4.00 to 4.90 wt% magnesium.
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Strength by temper
Minimum proof stress 125 to 215 MPa
Weight
2.65 g/cm³
Stiffness
72 GPa
Heat conduction
121 W/(m·K)
Welding
Arc and resistance welding rated excellent
Recipe, share of the weight
- Al balance (the rest)Aluminium
- Mg 4 to 4.9%Magnesium
- Mn 0.4 to 1%Manganese
- Cr 0.05 to 0.25%Chromium
- Fe max 0.40Iron
- Si max 0.40Silicon
- Cu max 0.10Copper
- Zn max 0.25Zinc
- Ti max 0.15Titanium
Best for
Welded marine structures and pressure vessels kept at or below 65 °C, where seawater resistance and strength matter (supplier datasheets)
Weakest at
Service above 65 °C, where the suppliers advise against use. It is a non-heat-treatable alloy (Dinco sheet). No space-environment data were found.
Risk at a glance
- People No data. No hazard data recorded
- If it fails No data. No failure risks recorded
- Corrosion Low. Highly resistant to attack by seawater and industrial chemicals (supplier sheets).
Quick facts: 5083
| Property | Value | Basis |
|---|---|---|
| Density | 2.65 g/cm³ | 1 sourced value |
| Yield strength | 125 to 215 MPa | 4 sourced values across conditions |
| Tensile strength | 275 to 385 MPa | 4 sourced values across conditions |
| Young's modulus | 72 GPa | 1 sourced value |
| Hardness (Brinell) | 75 to 89 HB | 3 sourced values across conditions |
| Thermal conductivity | 121 W/(m·K) | 1 sourced value |
| Thermal expansion (CTE) | 25 ppm/K | 1 sourced value |
| Melting point | 570 °C | 1 sourced value |
| Electrical resistivity | 5.8e-8 Ω·m | 1 sourced value |
What is the density of Aluminium alloy 5083?
Aluminium alloy 5083 has a density of 2.65 g/cm³. The source and test conditions are listed in the properties table on this page.
What is the thermal conductivity of Aluminium alloy 5083?
Aluminium alloy 5083 has a thermal conductivity of 121 W/(m·K). The source and test conditions are listed in the properties table on this page.
What is the coefficient of thermal expansion of Aluminium alloy 5083?
Aluminium alloy 5083 has a coefficient of thermal expansion of 25 ppm/K. The source and test conditions are listed in the properties table on this page.
What is the melting point of Aluminium alloy 5083?
Aluminium alloy 5083 has a melting point of 570 °C. The source and test conditions are listed in the properties table on this page.
What is the yield strength of Aluminium alloy 5083?
Aluminium alloy 5083 has a yield strength of 125 to 215 MPa. The range covers 4 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What are the other names and codes for Aluminium alloy 5083?
Aluminium alloy 5083 is also written as UNS A95083, EN 3.3547, EN name EN AW-5083, EN name AlMg4.5Mn0.7, AA 5083, AMS 4056. Each code is printed in the source listed beside it in the designations table.
What is Aluminium alloy 5083 used for?
Uses recorded in the sources include Ships and other marine structures; Pressure vessels; Rail cars, vehicle bodies, tipper truck bodies and mine skips and cages.
Why it exists
5083 is an aluminium-magnesium alloy sold for marine and pressure-vessel work. Magnesium, at 4.00 to 4.90 wt%, is the main addition. The Dinco sheet says the alloy has the highest strength of the non-heat-treatable aluminium alloys, is highly resistant to attack by seawater and industrial chemicals, and keeps its strength after welding. The suppliers list shipbuilding, pressure vessels, vehicle bodies and rail cars as typical uses, and they advise against use above 65 °C.
Where it's used
Ships and marine structures
The Dinco sheet, Smith Metal and AZoM all list shipbuilding. The Dinco sheet also lists marine applications and drilling rigs.
Pressure vessels
All three supplier pages list pressure vessels as a typical use.
Vehicle bodies, rail cars and mine skips
Smith Metal and AZoM list rail cars, vehicle bodies and tipper truck bodies, and both also list mine skips and cages.
Research on cryogenic hydrogen tanks
A 2007 Korean laboratory study tested aluminium alloys, including Al 5083, for automobile hydrogen storage tanks in liquid nitrogen. It is a laboratory study, not a product record.
Recipe
Al-Mg alloy; composition limits in wt% (Smith Metal datasheet): Mg 4.00 to 4.90, Mn 0.40 to 1.00, Cr 0.05 to 0.25, Fe max 0.40, Si max 0.40, Cu max 0.10, Zn max 0.25, Ti max 0.15, Al balance
5083 is a wrought aluminium-magnesium alloy. The Smith Metal datasheet gives magnesium at 4.00 to 4.90 wt% and manganese at 0.40 to 1.00 wt% as the main additions, with chromium at 0.05 to 0.25 wt% and small maximum limits for iron, silicon, copper, zinc and titanium. Aluminium is the balance. The Dinco sheet places the alloy among the non-heat-treatable alloys.
| Ingredient | Share of the weight | What it does |
|---|---|---|
| Aluminium Al | balance (the rest) | The matrix of the alloy; the balance after the alloying limits. |
| Magnesium Mg | 4 to 4.9% | Main alloying element, printed range 4.00 to 4.90 wt%. |
| Manganese Mn | 0.4 to 1% | Alloying addition inside the printed range; the sources read do not describe its function. |
| Chromium Cr | 0.05 to 0.25% | Minor addition inside the printed range; the sources read do not describe its function. |
| Iron Fe | max 0.40 | Limited to the printed maximum. |
| Silicon Si | max 0.40 | Limited to the printed maximum. |
| Copper Cu | max 0.10 | Limited to the printed maximum. |
| Zinc Zn | max 0.25 | Limited to the printed maximum. |
| Titanium Ti | max 0.15 | Limited to the printed maximum (the Dinco sheet prints 0.05 to 0.25). |
Weight shares are as printed in the sources.
What it can do
Strength by temper
Minimum proof stress 125 to 215 MPa
Minimum proof stress is 125 MPa for O/H111 sheet and 215 MPa for H32 sheet (BS EN 485-2 values on AZoM), and 195 MPa for H116 sheet and plate (Dinco). Tensile ranges printed are 275 to 350 MPa for O/H111 sheet, 305 to 380 MPa for H32 sheet and 305 to 385 MPa for H116.
Weight
2.65 g/cm³
measured
Density is 2.65 g/cm3, as printed by Smith Metal and Dinco.
Stiffness
72 GPa
measured
Modulus of elasticity is 72 GPa (Smith Metal).
Heat conduction
121 W/(m·K)
measured
Thermal conductivity is 121 W/(m·K) (Smith Metal).
Welding
Arc and resistance welding rated excellent
Arc and resistance welding are rated excellent and gas welding average. The alloy keeps its strength after welding (Dinco, Smith Metal, AZoM).
Seawater
Highly resistant
The suppliers rate the alloy highly resistant to attack by seawater and industrial chemicals (Dinco, Smith Metal, AZoM).
How it compares
5083 is a strong, weldable, seawater-resistant option for marine structures kept at or below 65 °C. The record holds no like-for-like figures for other alloys or for space use, so this profile does not rank it against other materials.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | 5083 | 6061 | 7075-T6 | 2024 | 5052 | 5XXX | 2195 (Al-Cu-Li) | Al | 1050 | 2011 | 2014 | 2017 | 2017A | 2219 | 2319 | 2618A | 3003 | 3103 | 4047 | 5019 | 5056 | AlMg2 | AlMg3 | 6013 | 6063 | 6082 | 6101 | AA7050 | AA8011 | Au-Al IMCs | Al master alloys |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Thermal behavior and safety | |||||||||||||||||||||||||||||||
| Melting point (one value printed) | 570 °C17 | no data | 532 °C | no data | 607.2 to 649 °C | no data | 1020 degF | 660 °C | 645 to 657 °C | 540 °C | 535 °C | 510 °C | 510 °C | 543 °C | 543 to 643 °C | 549 °C | 655 °C | 655 °C | 1068 to 1080 °F | 575 to 630 °C | 565 to 640 °C | 605 to 650 °C | 590 to 645 °C | 579 °C | 600 °C | 575 °C | 1090 °F | 490 °C | 640 to 655 °C | no data | 880 °C |
| Thermal conductivity | 121 W/(m·K)20 | 167 W/(m·K) | 130 W/m·K | 121 W/m-K | 138 W/m-K | 138 W/(m·K) | no data | 220 W/(m·K) | 229 W/m.K | 140 W/m.K | 138 W/(m·K) | 140 W/m.K | 140 W/m.K | 130 W.m/m2.°C | no data | 147 W/m.K | 190 W/m.K | 160 W/m.K | no data | 110 to 140 W/(m·K) | 109 to 117 W/(m·K) | 138 W/(m·K) | 140 to 160 W/(m·K) | 164 W/(m·K) | 200 W/(m·K) | 180 W/(m·K) | no data | 154 W/(m·K) | 210 to 220 W/(m·K) | no data | no data |
| Physical and electrical | |||||||||||||||||||||||||||||||
| Brinell hardness, O/H111 sheet 0.2 to 6.3 mm | 75 HB4 | no data | no data | no data | no data | no data | no data | no data | no data | no data | 138 HB | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | 52 HB | 130 HB | no data | 91 HB | no data | no data | no data | no data | no data |
| Vickers hardness, O/H111 (datasheet) | 75 HV9 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | 29 HV | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Brinell hardness, H32 sheet 0.2 to 6.00 mm | 89 HB12 | no data | no data | no data | no data | no data | no data | no data | no data | no data | 138 HB | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | 52 HB | 130 HB | no data | 91 HB | no data | no data | no data | no data | no data |
| Brinell hardness, H116Value printed on a supplier datasheet | 81 HB | no data | no data | no data | no data | no data | no data | no data | no data | no data | 138 HB | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | 52 HB | 130 HB | no data | 91 HB | no data | no data | no data | no data | no data |
| Density, printed as 2.65 g/cm³ | 2.65 g/cm³16 | 2.7 g/cm³ | 2.8 Mg/m3 | 2.78 g/cc | 2.68 g/cc | 2.68 g/cm³ | 0.096 lb/in3 | 2.7 g/cm³ | 2.71 g/cm³ | 2.82 g/cm³ | 2.82 g/cm³ | 2.79 g/cm³ | 2.79 g/cm³ | 2.84 g/cm³ | 2.84 g/cm³ | 2.76 g/cm³ | 2.73 g/cm³ | 2.73 g/cm³ | 2.65 g/cm³ | 2.64 g/cm³ | 2.64 g/cm³ | 2.69 g/cm³ | 2.67 g/cm³ | 2.71 g/cm³ | 2700 kg/m3 | 2.7 g/cm³ | 0.097 lb/cu.in | 2.83 g/cm³ | 2.71 g/cm³ | no data | no data |
| Electrical resistivity | 0.058 µΩ·m21 | 4 µΩ·cm | 5.2 µΩ·cm | 5.82 µΩ·cm | no data | 5.8 µΩ·cm | no data | 2.646 µΩ·cm | no data | no data | 0.045 µΩ·m | no data | no data | 5.7 μΩ.cm²/cm | no data | no data | no data | no data | no data | 0.0526 to 0.0667 Ω·mm²/m | 5.88×10^-8 to 6.25×10^-8 Ω·m | 50 nΩ·m | no data | no data | 0.35 µΩ·m | 0.038 µΩ·m | no data | no data | 2.86×10^-8 to 2.94×10^-8 Ω·m | no data | no data |
| Other measurements | |||||||||||||||||||||||||||||||
| Proof stress, minimum, O/H111 sheet 0.2 to 6.3 mm | > 125 MPa1 | 276 MPa | 503 MPa | 324 MPa | 13 ksi | 193 MPa | 74 ksi | 29 MPa | > 85 MPa | 140 MPa | > 400 MPa | 276 MPa | 276 MPa | > 50 ksi | 70 MPa | 350 MPa | 50 MPa | > 110 MPa | 55 MPa | no data | no data | > 120 MPa | > 80 MPa | 350 MPa | 21 ksi | > 255 MPa | 28000 psi | > 414 MPa | no data | no data | no data |
| Tensile strength, O/H111 sheet 0.2 to 6.3 mm | 275 to 350 MPa2 | 310 MPa | 572 MPa | 469 MPa | 28 ksi | 228 MPa | 80 ksi | 88 MPa | 105 to 145 MPa | 300 MPa | > 460 MPa | 427 MPa | 427 MPa | > 62 ksi | 160 MPa | 420 MPa | 110 MPa | > 140 MPa | 124 MPa | 270 to 350 MPa | 300 MPa | 190 to 230 MPa | 190 to 260 MPa | 410 MPa | 27 ksi | > 300 MPa | 32000 psi | > 483 MPa | 180 to 195 MPa | no data | no data |
| Elongation A, O/H111 plate 80 to 120 mm | > 12 %3 | 17 % | 11 % | 19 % | 25 % | 12 % | 8 % | 50 to 65 % | 4 to 8 % | 16 % | > 6 % | 18 % | 18 % | > 6 % | 12 % | > 5 % | 25 % | > 8 % | 12 % | > 2 % | 20 % | 4 to 12 % | > 12 % | 4 % | 8 % | > 9 % | > 8 % | > 7 % | > 1 % | no data | no data |
| Proof stress, O/H111 (datasheet) | 145 MPa5 | 276 MPa | 503 MPa | 324 MPa | 13 ksi | 193 MPa | 74 ksi | 29 MPa | > 85 MPa | 140 MPa | > 400 MPa | 276 MPa | 276 MPa | > 50 ksi | 70 MPa | 350 MPa | 50 MPa | > 110 MPa | 55 MPa | no data | no data | > 120 MPa | > 80 MPa | 350 MPa | 21 ksi | > 255 MPa | 28000 psi | > 414 MPa | no data | no data | no data |
| Tensile strength, O/H111 (datasheet) | 300 MPa6 | 310 MPa | 572 MPa | 469 MPa | 28 ksi | 228 MPa | 80 ksi | 88 MPa | 105 to 145 MPa | 300 MPa | > 460 MPa | 427 MPa | 427 MPa | > 62 ksi | 160 MPa | 420 MPa | 110 MPa | > 140 MPa | 124 MPa | 270 to 350 MPa | 300 MPa | 190 to 230 MPa | 190 to 260 MPa | 410 MPa | 27 ksi | > 300 MPa | 32000 psi | > 483 MPa | 180 to 195 MPa | no data | no data |
| Elongation A50, O/H111 (datasheet) | 23 %7 | 17 % | 11 % | 19 % | 25 % | 12 % | 8 % | 50 to 65 % | 4 to 8 % | 16 % | > 6 % | 18 % | 18 % | > 6 % | 12 % | > 5 % | 25 % | > 8 % | 12 % | > 2 % | 20 % | 4 to 12 % | > 12 % | 4 % | 8 % | > 9 % | > 8 % | > 7 % | > 1 % | no data | no data |
| Shear strength, O/H111 (datasheet) | 175 MPa8 | no data | no data | no data | no data | no data | no data | no data | 70 N/mm2 | no data | no data | no data | no data | no data | no data | 260 MPa | 75 MPa | 90 MPa | no data | no data | no data | no data | no data | 240 MPa | no data | no data | no data | no data | no data | no data | no data |
| Proof stress, minimum, H32 sheet 0.2 to 6.00 mm | > 215 MPa10 | 276 MPa | 503 MPa | 324 MPa | 13 ksi | 193 MPa | 74 ksi | 29 MPa | > 85 MPa | 140 MPa | > 400 MPa | 276 MPa | 276 MPa | > 50 ksi | 70 MPa | 350 MPa | 50 MPa | > 110 MPa | 55 MPa | no data | no data | > 120 MPa | > 80 MPa | 350 MPa | 21 ksi | > 255 MPa | 28000 psi | > 414 MPa | no data | no data | no data |
| Tensile strength, H32 sheet 0.2 to 6.00 mm | 305 to 380 MPa11 | 310 MPa | 572 MPa | 469 MPa | 28 ksi | 228 MPa | 80 ksi | 88 MPa | 105 to 145 MPa | 300 MPa | > 460 MPa | 427 MPa | 427 MPa | > 62 ksi | 160 MPa | 420 MPa | 110 MPa | > 140 MPa | 124 MPa | 270 to 350 MPa | 300 MPa | 190 to 230 MPa | 190 to 260 MPa | 410 MPa | 27 ksi | > 300 MPa | 32000 psi | > 483 MPa | 180 to 195 MPa | no data | no data |
| Proof stress, minimum, H116 sheet and plateMinimum value printed on a supplier datasheet | > 195 MPa13 | 276 MPa | 503 MPa | 324 MPa | 13 ksi | 193 MPa | 74 ksi | 29 MPa | > 85 MPa | 140 MPa | > 400 MPa | 276 MPa | 276 MPa | > 50 ksi | 70 MPa | 350 MPa | 50 MPa | > 110 MPa | 55 MPa | no data | no data | > 120 MPa | > 80 MPa | 350 MPa | 21 ksi | > 255 MPa | 28000 psi | > 414 MPa | no data | no data | no data |
| Tensile strength, H116 sheet and plateRange printed on a supplier datasheet | 305 to 385 MPa14 | 310 MPa | 572 MPa | 469 MPa | 28 ksi | 228 MPa | 80 ksi | 88 MPa | 105 to 145 MPa | 300 MPa | > 460 MPa | 427 MPa | 427 MPa | > 62 ksi | 160 MPa | 420 MPa | 110 MPa | > 140 MPa | 124 MPa | 270 to 350 MPa | 300 MPa | 190 to 230 MPa | 190 to 260 MPa | 410 MPa | 27 ksi | > 300 MPa | 32000 psi | > 483 MPa | 180 to 195 MPa | no data | no data |
| Elongation at 50 mm, H116 (minimum)Minimum value printed on a supplier datasheet | > 8 %15 | 17 % | 11 % | 19 % | 25 % | 12 % | 8 % | 50 to 65 % | 4 to 8 % | 16 % | > 6 % | 18 % | 18 % | > 6 % | 12 % | > 5 % | 25 % | > 8 % | 12 % | > 2 % | 20 % | 4 to 12 % | > 12 % | 4 % | 8 % | > 9 % | > 8 % | > 7 % | > 1 % | no data | no data |
| Thermal expansion coefficient | 25 ppm/K18 | 23.6 ppm/K | 23.4 µm/m·K | 23.2 ppm/K | 24.8 µm/m-°C | 24 ppm/K | no data | 22.5 ppm/K | 23.5 x10-6/K | 21.4 µm/m.°C | 23 ppm/K | 22.9 µm/(m·°C) | 22.9 µm/m.°C | 22.5 x10^-6 m/m.°C | no data | 21.6 µm/m°C | 23.1 ppm/K | 23.1 x10-6/K | no data | no data | 2.41×10^-5 1/K | 23.8 µm/m/°C | 23.9 ppm/K | 21.7 µm/m°C | 23.5 ppm/K | 23.1 ppm/K | no data | 23.5 ppm/K | 2.35×10^-5 1/K | no data | no data |
| Modulus of elasticity | 72 GPa19 | 68.9 GPa | 71 GPa | 73.1 GPa | 70.3 GPa | 70.3 GPa | 11 MSI | 69 GPa | 69000 MPa | 70 GPa | 71 GPa | 72 GPa | 72 GPa | 73.8 x10^3 N/mm2 | no data | 71 GPa | 69.5 GPa | 69.5 GPa | no data | 70 GPa | 71 GPa | 70 GPa | 70 GPa | 71 GPa | 69.5 GPa | 70 GPa | no data | 71.5 GPa | 70 GPa | no data | no data |
Why choose it, and why not
Good for
- Marine structures and ships, where the suppliers cite seawater resistance and good weldability (Dinco, Smith Metal, AZoM).
- Pressure vessels kept at or below 65 °C (Dinco, Smith Metal, AZoM).
- Rail cars and vehicle bodies, which the suppliers list as typical uses (Smith Metal, AZoM).
- Low-temperature service: the Smith Metal product page says the alloy performs well at low temperature. No numbers are printed.
Watch out for
- Service above 65 °C. The suppliers say not to use the alloy there.
- Long exposure to liquid nitrogen lowered the elongation of 5083 in a 2007 laboratory study.
- Strength values come from supplier and distributor pages for O/H111, H32 and H116, and some are minimum values. H321 values, ASTM designations and space data were not found.
5083 is a weldable marine aluminium alloy with supplier-rated seawater resistance and a 65 °C service limit. The record leaves out the H321 marine temper, the ASTM designations, exfoliation data and any space-environment data.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Other names and standards
The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.
| System | Codes |
|---|---|
| UNS | A95083 |
| EN | 3.3547 |
| EN name | EN AW-5083, AlMg4.5Mn0.7 |
| AA | 5083 |
| AMS | 4056 |
| MIL | MIL-A-46027 |
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Proof stress, minimum, O/H111 sheet 0.2 to 6.3 mm | Minimum value in a mechanical-properties table on a web article that quotes supplier data | temper O/H111 (the table prints one set for both tempers)product form sheet, 0.2 to 6.3 mmstandard BS EN 485-2:2008, as printedoffset not printedbasis minimum value in the table | The table does not separate O from H111, and the proof-stress offset is not printed. |
| 2 | Tensile strength, O/H111 sheet 0.2 to 6.3 mm | Range in a mechanical-properties table on a web article that quotes supplier data | temper O/H111 (one set for both tempers)product form sheet, 0.2 to 6.3 mmstandard BS EN 485-2:2008, as printed | — |
| 3 | Elongation A, O/H111 plate 80 to 120 mm | Minimum value in a mechanical-properties table on a web article that quotes supplier data | temper O/H111product form plate, 80 to 120 mmstandard BS EN 485-2:2008, as printedgauge length not printed | — |
| 4 | Brinell hardness, O/H111 sheet 0.2 to 6.3 mm | Value in a mechanical-properties table on a web article that quotes supplier data | temper O/H111 (one set for both tempers)product form sheet, 0.2 to 6.3 mm | — |
| 5 | Proof stress, O/H111 (datasheet) | Value in a mechanical-properties table of a supplier datasheet | temper O/H111 (the datasheet says its values are for O/H111)basis printed without a minimum or typical markingoffset not printedproduct form not stated | The datasheet gives one set for O and H111 and does not mark the value as minimum or typical. |
| 6 | Tensile strength, O/H111 (datasheet) | Value in a mechanical-properties table of a supplier datasheet | temper O/H111 (the datasheet says its values are for O/H111)basis printed without a minimum or typical marking | — |
| 7 | Elongation A50, O/H111 (datasheet) | Value in a mechanical-properties table of a supplier datasheet | temper O/H111 (the datasheet says its values are for O/H111)gauge length 50 mmbasis printed without a minimum or typical marking | — |
| 8 | Shear strength, O/H111 (datasheet) | Value in a mechanical-properties table of a supplier datasheet; the name is not in the property list | temper O/H111 (the datasheet says its values are for O/H111)basis printed without a minimum or typical marking | — |
| 9 | Vickers hardness, O/H111 (datasheet) | Value in a mechanical-properties table of a supplier datasheet; the name is not in the property list | temper O/H111 (the datasheet says its values are for O/H111) | — |
| 10 | Proof stress, minimum, H32 sheet 0.2 to 6.00 mm | Minimum value in a mechanical-properties table on a web article that quotes supplier data | temper H32 (described on the same page as quarter hard)product form sheet, 0.2 to 6.00 mmstandard BS EN 485-2:2008, as printedoffset not printed | — |
| 11 | Tensile strength, H32 sheet 0.2 to 6.00 mm | Range in a mechanical-properties table on a web article that quotes supplier data | temper H32product form sheet, 0.2 to 6.00 mmstandard BS EN 485-2:2008, as printed | — |
| 12 | Brinell hardness, H32 sheet 0.2 to 6.00 mm | Value in a mechanical-properties table on a web article that quotes supplier data | temper H32product form sheet, 0.2 to 6.00 mm | — |
| 13 | Proof stress, minimum, H116 sheet and plate | — | temper H116product form sheet and plate with DNV class certification, as offered by the supplieroffset not printedbasis minimum value printed on the datasheetunit in source Mpa | — |
| 14 | Tensile strength, H116 sheet and plate | — | temper H116product form sheet and plate, as offered by the supplierunit in source Mpa | — |
| 15 | Elongation at 50 mm, H116 (minimum) | — | temper H116gauge length 50 mmbasis minimum value printed on the datasheet | — |
| 16 | Density, printed as 2.65 g/cm³ | Value in the physical-properties table of a supplier datasheet for 5083 | temper not statedtemperature not stated | — |
| 17 | Melting point (one value printed) | Value in the physical-properties table of a supplier datasheet for 5083 | temper not statedbasis one value printed; solidus and liquidus not printed | The datasheet prints one value, not a melting range. |
| 18 | Thermal expansion coefficient | Value in the physical-properties table of a supplier datasheet for 5083; printed as 10-6/K and written here as ppm/K (same unit) | temper not statedtemperature range not statedunit in source x10-6 /K, equal to ppm/K | — |
| 19 | Modulus of elasticity | Value in the physical-properties table of a supplier datasheet for 5083 | temper not statedtemperature not stated | — |
| 20 | Thermal conductivity | Value in the physical-properties table of a supplier datasheet for 5083; printed as W/m.K and written here as W/(m·K) (same unit) | temper not statedtemperature not statedunit in source W/m.K | — |
| 21 | Electrical resistivity | Value in the physical-properties table of the H116 datasheet for 5083; printed as 0.058 x 10-6 Ω.m and written here as 0.058 µΩ·m (the 10-6 factor is the µ prefix) | temper not statedtemperature not statedunit in source 0.058 x 10-6 Ω.m | AZoM prints 0.58 x 10-6 Ω.m for the same property, ten times this value. That printed value is not recorded here. |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Sea water and industrial chemicals | low | Highly resistant to attack by seawater and industrial chemicals (supplier sheets).1 |
| Service above 65 °C | not rated | Suppliers advise against use above 65 °C.2 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Sea water and industrial chemicals | The Dinco sheet says the alloy is highly resistant to attack by both seawater and industrial chemical environments. Smith Metal and AZoM give the same description. No exposure time, test method or corrosion rate is printed in the sources read. | basis general statements on supplier sheets; no exposure test data printed |
| 2 | Service above 65 °C | The Dinco sheet says the alloy is not recommended for use in temperatures in excess of 65 °C. Smith Metal says it is not recommended above 65 °C, and AZoM repeats the limit. None of the sources read names sensitisation or intergranular attack as the reason. | temperature limit 65 °C (as printed) |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
No safety data sheet for the alloy was read in this run. The hazard entries are PubChem's element-level data for aluminium, magnesium and manganese.
- What the sources cover
- The sources read describe the metals' flammability and water reactivity as classified in PubChem's company reports, and the suppliers' corrosion and welding behaviour. They do not describe health effects of the alloy.
- Not covered
- Hazard classification for 5083 as supplied, and for dust or fume from cutting or welding, was not found in a source read in this run.
If it fails
These are the failure routes named in the sources. They are supplier statements and laboratory results, not field incident data.
- Use above 65 °C
- The suppliers say not to use the alloy above 65 °C. The sources read do not say what happens above that limit.
- Long exposure to liquid nitrogen
- In a 2007 laboratory study, the elongation of Al 5083 at cryogenic temperature fell with longer immersion in liquid nitrogen. The abstract attributes this to non-uniform fracture of precipitates on grain boundaries.
Handling and welding
- Welding
- Arc and resistance welding are rated excellent and gas welding average. Brazing is rated poor. AZoM recommends filler 5183 for welding 5083 to itself.
- Machining
- Machinability is rated poor, and cold workability average.
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Use above 65 °C | Service temperature above 65 °CThe suppliers say not to use the alloy above 65 °C. The sources read do not say what happens above that limit. |
| Lower elongation after long exposure to liquid nitrogen | Holding the alloy in liquid nitrogen for longer times (laboratory test, 2007)The abstract says the elongation of Al 5083 at cryogenic temperature decreased with longer immersion, because of non-uniform fracture of precipitates on grain boundaries. The same abstract says Al 6061 kept its elongation regardless of immersion time. |
Handling and storage
- Weldability as rated on the Dinco sheet: gas welding average, arc welding excellent, resistance welding excellent, brazing poor.
- AZoM's fabrication table rates weldability gas average, arc excellent and resistance excellent; brazability and solderability poor; machinability poor; cold workability average.
- AZoM recommends filler 5183 for welding 5083 to itself or to another alloy of the same sub-group; 5356 and 5556 are other suitable fillers.
- Smith Metal's datasheet says 5083 retains exceptional strength after welding.
- Smith Metal's product page says the alloy combines excellent ductility with good formability and performs well in low-temperature service.
- Machinability is rated poor on the Dinco sheet and in AZoM's Table 4.
Mitigations
- Keep service at or below 65 °C, the limit printed by the suppliers.
Supply and geography
How common the raw materials are and where they come from.
Aluminium (primary smelter production)
- Top producers (2025)
- China 60.8%, India 5.7%, Russia 5.3%, Canada 4.5%, United Arab Emirates 3.6%
- Critical mineral lists
- US: listed, EU: listed
- Recycling
- USGS: in 2025 about 3.6 million tons of aluminum was recovered from purchased scrap in the United States.
- Substitutes
- USGS: composites, magnesium, steel and titanium can substitute for aluminum in ground transportation uses.
Bauxite (aluminium ore)
- Top producers (2025)
- Guinea 34.1%, Australia 22%, China 19.8%, Brazil 7.5%, India 5.7%
- Critical mineral lists
- EU: listed
- Recycling
- USGS bauxite and alumina chapter: 'None.'
- Substitutes
- USGS: bauxite is the only raw material used to produce alumina on a commercial scale in the United States; clay is technically feasible but not currently economically competitive.
Alumina (aluminium oxide)
- Top producers (2025)
- China 62%, Australia 11.3%, Brazil 7.3%, India 5.5%, Russia 1.9%
- Recycling
- USGS bauxite and alumina chapter: 'None.'
- Substitutes
- USGS: other raw materials such as alunite, anorthosite, coal wastes and oil shales offer potential alumina sources.
Magnesium (metal)
- Top producers (2025)
- China 86.4%, Russia 5.5%, Brazil 1.8%, Israel 1.8%, Turkey 1.4%
- Critical mineral lists
- US: listed, EU: listed
- Recycling
- USGS: in 2025 about 26,000 tons of secondary magnesium was recovered from old scrap and 82,000 tons from new scrap.
- Substitutes
- USGS: aluminum and zinc may substitute for magnesium in castings and wrought products; magnesium's lower weight is an advantage, but its high cost is a disadvantage.
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: aluminium-5083
spore_version: 0.2
family: aluminium-alloys
name: Aluminium alloy 5083
abbreviation: '5083'
role: marine structural alloy
category: metals
type: aluminium
summary: 5083 is a wrought aluminium-magnesium alloy with 4.00 to 4.90 wt% magnesium. Its suppliers describe it as the strongest of the non-heat-treatable aluminium alloys and as highly resistant to attack by seawater and industrial chemicals. It is used for ships, pressure vessels, vehicle bodies and rail cars, and the suppliers advise against use above 65 °C.
best_for: Welded marine structures and pressure vessels kept at or below 65 °C, where seawater resistance and strength matter (supplier datasheets)
weakest_at: Service above 65 °C, where the suppliers advise against use. It is a non-heat-treatable alloy (Dinco sheet). No space-environment data were found.
identity:
formula: 'Al-Mg alloy; composition limits in wt% (Smith Metal datasheet): Mg 4.00 to 4.90, Mn 0.40 to 1.00, Cr 0.05 to 0.25, Fe max 0.40, Si max 0.40, Cu max 0.10, Zn max 0.25, Ti max 0.15, Al balance'
source: smith-5083-datasheet
where: Chemical Composition (weight %) table
designations:
- system: UNS
code: A95083
source: nist-5083
where: 'Page title line, Material Properties: 5083 Aluminum (UNS A95083)'
- system: EN
code: '3.3547'
source: alloysintl-5083
where: Designations and cross reference table, Werkstoff (W.Nr) 3.3547
- system: EN name
code: EN AW-5083
source: alloysintl-5083
where: Designations and cross reference table, EN designation line
- system: EN name
code: AlMg4.5Mn0.7
source: alloysintl-5083
where: Same EN designation line, after the slash
- system: AA
code: '5083'
source: dinco-5083h116
where: Title line, Aluminium Alloy AA 5083 H116 Data Sheet
- system: AMS
code: '4056'
source: alloysintl-5083
where: Specifications list on the 5083 grade page (product form not printed)
- system: MIL
code: MIL-A-46027
source: alloysintl-5083
where: Specifications list on the 5083 grade page (product form not printed)
tags:
environments: []
stresses:
- extreme-cold
applications:
- structures
- propulsion-and-tanks
- cryogenic-fuel
properties:
- benchmark: yield_strength
label: Proof stress, minimum, O/H111 sheet 0.2 to 6.3 mm
value: 125
bound: lower
unit: MPa
scope: material
conditions:
temper: O/H111 (the table prints one set for both tempers)
product_form: sheet, 0.2 to 6.3 mm
standard: BS EN 485-2:2008, as printed
offset: not printed
basis: minimum value in the table
method: Minimum value in a mechanical-properties table on a web article that quotes supplier data
status: ground
note: The table does not separate O from H111, and the proof-stress offset is not printed.
source: azom-aalco-5083
where: Table 2 (a), row Proof Stress
- benchmark: ultimate_tensile_strength
label: Tensile strength, O/H111 sheet 0.2 to 6.3 mm
value: 275
value_high: 350
bound: range
unit: MPa
scope: material
conditions:
temper: O/H111 (one set for both tempers)
product_form: sheet, 0.2 to 6.3 mm
standard: BS EN 485-2:2008, as printed
method: Range in a mechanical-properties table on a web article that quotes supplier data
status: ground
source: azom-aalco-5083
where: Table 2 (a), row Tensile Strength
- benchmark: elongation
label: Elongation A, O/H111 plate 80 to 120 mm
value: 12
bound: lower
unit: '%'
scope: material
conditions:
temper: O/H111
product_form: plate, 80 to 120 mm
standard: BS EN 485-2:2008, as printed
gauge_length: not printed
method: Minimum value in a mechanical-properties table on a web article that quotes supplier data
status: ground
source: azom-aalco-5083
where: Table 2 (c), row Elongation A
- benchmark: hardness_brinell
label: Brinell hardness, O/H111 sheet 0.2 to 6.3 mm
value: 75
unit: HB
scope: material
conditions:
temper: O/H111 (one set for both tempers)
product_form: sheet, 0.2 to 6.3 mm
method: Value in a mechanical-properties table on a web article that quotes supplier data
status: ground
source: azom-aalco-5083
where: Table 2 (a), row Hardness Brinell
- benchmark: yield_strength
label: Proof stress, O/H111 (datasheet)
value: 145
unit: MPa
scope: material
conditions:
temper: O/H111 (the datasheet says its values are for O/H111)
basis: printed without a minimum or typical marking
offset: not printed
product_form: not stated
method: Value in a mechanical-properties table of a supplier datasheet
status: ground
note: The datasheet gives one set for O and H111 and does not mark the value as minimum or typical.
source: smith-5083-datasheet
where: Mechanical Properties table, Proof Stress
- benchmark: ultimate_tensile_strength
label: Tensile strength, O/H111 (datasheet)
value: 300
unit: MPa
scope: material
conditions:
temper: O/H111 (the datasheet says its values are for O/H111)
basis: printed without a minimum or typical marking
method: Value in a mechanical-properties table of a supplier datasheet
status: ground
source: smith-5083-datasheet
where: Mechanical Properties table, Tensile Strength
- benchmark: elongation
label: Elongation A50, O/H111 (datasheet)
value: 23
unit: '%'
scope: material
conditions:
temper: O/H111 (the datasheet says its values are for O/H111)
gauge_length: 50 mm
basis: printed without a minimum or typical marking
method: Value in a mechanical-properties table of a supplier datasheet
status: ground
source: smith-5083-datasheet
where: Mechanical Properties table, Elongation A50 mm
- benchmark: shear_strength
label: Shear strength, O/H111 (datasheet)
value: 175
unit: MPa
scope: material
conditions:
temper: O/H111 (the datasheet says its values are for O/H111)
basis: printed without a minimum or typical marking
method: Value in a mechanical-properties table of a supplier datasheet; the name is not in the property list
status: ground
source: smith-5083-datasheet
where: Mechanical Properties table, Shear Strength
- benchmark: hardness_vickers
label: Vickers hardness, O/H111 (datasheet)
value: 75
unit: HV
scope: material
conditions:
temper: O/H111 (the datasheet says its values are for O/H111)
method: Value in a mechanical-properties table of a supplier datasheet; the name is not in the property list
status: ground
source: smith-5083-datasheet
where: Mechanical Properties table, Hardness Vickers
- benchmark: yield_strength
label: Proof stress, minimum, H32 sheet 0.2 to 6.00 mm
value: 215
bound: lower
unit: MPa
scope: material
conditions:
temper: H32 (described on the same page as quarter hard)
product_form: sheet, 0.2 to 6.00 mm
standard: BS EN 485-2:2008, as printed
offset: not printed
method: Minimum value in a mechanical-properties table on a web article that quotes supplier data
status: ground
source: azom-aalco-5083
where: Table 2 (d), row Proof Stress
- benchmark: ultimate_tensile_strength
label: Tensile strength, H32 sheet 0.2 to 6.00 mm
value: 305
value_high: 380
bound: range
unit: MPa
scope: material
conditions:
temper: H32
product_form: sheet, 0.2 to 6.00 mm
standard: BS EN 485-2:2008, as printed
method: Range in a mechanical-properties table on a web article that quotes supplier data
status: ground
source: azom-aalco-5083
where: Table 2 (d), row Tensile Strength
- benchmark: hardness_brinell
label: Brinell hardness, H32 sheet 0.2 to 6.00 mm
value: 89
unit: HB
scope: material
conditions:
temper: H32
product_form: sheet, 0.2 to 6.00 mm
method: Value in a mechanical-properties table on a web article that quotes supplier data
status: ground
source: azom-aalco-5083
where: Table 2 (d), row Hardness Brinell
- benchmark: yield_strength
label: Proof stress, minimum, H116 sheet and plate
value: 195
bound: lower
unit: MPa
scope: material
conditions:
temper: H116
product_form: sheet and plate with DNV class certification, as offered by the supplier
offset: not printed
basis: minimum value printed on the datasheet
unit_in_source: Mpa
method: Minimum value printed on a supplier datasheet
status: ground
source: dinco-5083h116
where: Mechanical Properties table, Proof Stress (195 Min)
- benchmark: ultimate_tensile_strength
label: Tensile strength, H116 sheet and plate
value: 305
value_high: 385
bound: range
unit: MPa
scope: material
conditions:
temper: H116
product_form: sheet and plate, as offered by the supplier
unit_in_source: Mpa
method: Range printed on a supplier datasheet
status: ground
source: dinco-5083h116
where: Mechanical Properties table, Tensile Strength
- benchmark: elongation
label: Elongation at 50 mm, H116 (minimum)
value: 8
bound: lower
unit: '%'
scope: material
conditions:
temper: H116
gauge_length: 50 mm
basis: minimum value printed on the datasheet
method: Minimum value printed on a supplier datasheet
status: ground
source: dinco-5083h116
where: Mechanical Properties table, Elongation at 50 mm (8 Min)
- benchmark: hardness_brinell
label: Brinell hardness, H116
value: 81
unit: HB
scope: material
conditions:
temper: H116
method: Value printed on a supplier datasheet
status: ground
source: dinco-5083h116
where: Mechanical Properties table, Hardness Brinell
- benchmark: density
label: Density, printed as 2.65 g/cm³
value: 2.65
unit: g/cm3
scope: material
conditions:
temper: not stated
temperature: not stated
method: Value in the physical-properties table of a supplier datasheet for 5083
status: ground
source: smith-5083-datasheet
where: Physical Properties table, Density (2.65 g/cm³)
- benchmark: melting_point
label: Melting point (one value printed)
value: 570
unit: °C
scope: material
conditions:
temper: not stated
basis: one value printed; solidus and liquidus not printed
method: Value in the physical-properties table of a supplier datasheet for 5083
status: ground
note: The datasheet prints one value, not a melting range.
source: smith-5083-datasheet
where: Physical Properties table, Melting Point
- benchmark: cte
label: Thermal expansion coefficient
value: 25
unit: ppm/K
scope: material
conditions:
temper: not stated
temperature_range: not stated
unit_in_source: x10-6 /K, equal to ppm/K
method: Value in the physical-properties table of a supplier datasheet for 5083; printed as 10-6/K and written here as ppm/K (same unit)
status: ground
source: smith-5083-datasheet
where: Physical Properties table, Thermal Expansion
- benchmark: elastic_modulus
label: Modulus of elasticity
value: 72
unit: GPa
scope: material
conditions:
temper: not stated
temperature: not stated
method: Value in the physical-properties table of a supplier datasheet for 5083
status: ground
source: smith-5083-datasheet
where: Physical Properties table, Modulus of Elasticity
- benchmark: thermal_conductivity
label: Thermal conductivity
value: 121
unit: W/(m·K)
scope: material
conditions:
temper: not stated
temperature: not stated
unit_in_source: W/m.K
method: Value in the physical-properties table of a supplier datasheet for 5083; printed as W/m.K and written here as W/(m·K) (same unit)
status: ground
source: smith-5083-datasheet
where: Physical Properties table, Thermal Conductivity
- benchmark: electrical_resistivity
label: Electrical resistivity
value: 0.058
unit: µΩ·m
scope: material
conditions:
temper: not stated
temperature: not stated
unit_in_source: 0.058 x 10-6 Ω.m
method: Value in the physical-properties table of the H116 datasheet for 5083; printed as 0.058 x 10-6 Ω.m and written here as 0.058 µΩ·m (the 10-6 factor is the µ prefix)
status: ground
note: AZoM prints 0.58 x 10-6 Ω.m for the same property, ten times this value. That printed value is not recorded here.
source: dinco-5083h116
where: Physical properties table, Electrical Resistivity
corrosion:
- environment: Sea water and industrial chemicals
headline: Highly resistant to attack by seawater and industrial chemicals (supplier sheets).
effect: The Dinco sheet says the alloy is highly resistant to attack by both seawater and industrial chemical environments. Smith Metal and AZoM give the same description. No exposure time, test method or corrosion rate is printed in the sources read.
rating: low
conditions:
basis: general statements on supplier sheets; no exposure test data printed
source: dinco-5083h116
where: Description paragraph
- environment: Service above 65 °C
headline: Suppliers advise against use above 65 °C.
effect: The Dinco sheet says the alloy is not recommended for use in temperatures in excess of 65 °C. Smith Metal says it is not recommended above 65 °C, and AZoM repeats the limit. None of the sources read names sensitisation or intergranular attack as the reason.
rating: unknown
conditions:
temperature_limit: 65 °C (as printed)
source: dinco-5083h116
where: Description paragraph
risks:
hazards:
- text: PubChem's aggregated GHS reports for aluminium metal (4,079 reports from companies, 35 notifications) give H261 in 90.8% of reports (in contact with water releases flammable gas), H228 in 60.6% (flammable solid) and H250 in 34.2% (catches fire spontaneously if exposed to air). These are element-level statements, not a classification of the alloy.
ghs:
- H261
- H228
- H250
source: pubchem-al
where: Safety and Hazards, GHS Classification (CID 5359268)
- text: PubChem's aggregated GHS reports for magnesium metal (2,205 reports from companies, 27 notifications) give H228 in 44.9%, H261 in 44.8%, H260 in 36.7%, H250 in 36.5% and H252 in 18%. These are element-level statements, not a classification of the alloy.
ghs:
- H228
- H261
- H260
- H250
- H252
source: pubchem-mg
where: Safety and Hazards, GHS Classification (CID 5462224)
- text: PubChem's aggregated GHS reports for manganese (3,101 reports from companies, 22 notifications) give H319 in 14.8%, H228 in 11.6%, H411 in 10.9% and H412 in 10.8%. Other notifications list H360 and H372 without a percentage. These are element-level statements, not a classification of the alloy.
ghs:
- H319
- H228
- H411
- H412
- H360
- H372
source: pubchem-mn
where: Safety and Hazards, GHS Classification (CID 23930)
failure_risks:
- mode: Use above 65 °C
trigger: Service temperature above 65 °C
consequence: The suppliers say not to use the alloy above 65 °C. The sources read do not say what happens above that limit.
source: dinco-5083h116
where: Description paragraph
- mode: Lower elongation after long exposure to liquid nitrogen
trigger: Holding the alloy in liquid nitrogen for longer times (laboratory test, 2007)
consequence: The abstract says the elongation of Al 5083 at cryogenic temperature decreased with longer immersion, because of non-uniform fracture of precipitates on grain boundaries. The same abstract says Al 6061 kept its elongation regardless of immersion time.
source: koreascience-2007
where: Abstract
side_effects: []
handling:
- text: 'Weldability as rated on the Dinco sheet: gas welding average, arc welding excellent, resistance welding excellent, brazing poor.'
source: dinco-5083h116
where: Weldability and Brazability entries
- text: AZoM's fabrication table rates weldability gas average, arc excellent and resistance excellent; brazability and solderability poor; machinability poor; cold workability average.
source: azom-aalco-5083
where: Table 4, Fabrication response
- text: AZoM recommends filler 5183 for welding 5083 to itself or to another alloy of the same sub-group; 5356 and 5556 are other suitable fillers.
source: azom-aalco-5083
where: Fabrication of Aluminium Alloy 5083, Welding
- text: Smith Metal's datasheet says 5083 retains exceptional strength after welding.
source: smith-5083-datasheet
where: Weldability section
- text: Smith Metal's product page says the alloy combines excellent ductility with good formability and performs well in low-temperature service.
source: smith-5083-page
where: Product description, Good Weldability section
- text: Machinability is rated poor on the Dinco sheet and in AZoM's Table 4.
source: dinco-5083h116
where: Fabrication entry, Machinability
mitigations:
- text: Keep service at or below 65 °C, the limit printed by the suppliers.
source: dinco-5083h116
where: Description paragraph
uses:
- application: structures
device: Ships and other marine structures
example: The Dinco sheet lists ship building and marine applications; Smith Metal and AZoM list shipbuilding.
source: dinco-5083h116
where: Applications list
- application: propulsion-and-tanks
device: Pressure vessels
example: Listed as a typical use by the Dinco sheet, Smith Metal and AZoM.
source: dinco-5083h116
where: Applications list
- application: structures
device: Rail cars, vehicle bodies, tipper truck bodies and mine skips and cages
example: Smith Metal and AZoM list rail cars, vehicle bodies and tipper or tip truck bodies, and mine skips and cages.
source: smith-5083-datasheet
where: Applications list
- application: cryogenic-fuel
device: Hydrogen storage tank for an automobile, tested in liquid nitrogen (laboratory study, not a product record)
example: The 2007 study's abstract says the aluminium alloys it tested, including Al 5083, are used for hydrogen storage tanks of automobiles at cryogenic temperature.
source: koreascience-2007
where: Abstract
supply:
- subject: Aluminium (primary smelter production)
producers:
- country: China
share_percent: 60.8
year: 2025
- country: India
share_percent: 5.7
year: 2025
- country: Russia
share_percent: 5.3
year: 2025
- country: Canada
share_percent: 4.5
year: 2025
- country: United Arab Emirates
share_percent: 3.6
year: 2025
critical_lists:
- list: USGS 2025 List of Critical Minerals (listed as Aluminum)
listed: true
- list: EU list of 34 critical raw materials (the EC page says aluminium and bauxite have been merged)
listed: true
recycling: 'USGS: in 2025 about 3.6 million tons of aluminum was recovered from purchased scrap in the United States.'
substitutes:
- 'USGS: composites, magnesium, steel and titanium can substitute for aluminum in ground transportation uses.'
source: usgs-mcs2026-aluminum
where: 'World Smelter Production table, 2025e (world total 74,000 thousand t; shares calculated here from the printed tonnes); Recycling; Substitutes. Lists: see sources usgs-crit2025 and ec-crm'
- subject: Bauxite (aluminium ore)
producers:
- country: Guinea
share_percent: 34.1
year: 2025
- country: Australia
share_percent: 22
year: 2025
- country: China
share_percent: 19.8
year: 2025
- country: Brazil
share_percent: 7.5
year: 2025
- country: India
share_percent: 5.7
year: 2025
critical_lists:
- list: EU list of 34 critical raw materials (Bauxite listed)
listed: true
recycling: 'USGS bauxite and alumina chapter: ''None.'''
substitutes:
- 'USGS: bauxite is the only raw material used to produce alumina on a commercial scale in the United States; clay is technically feasible but not currently economically competitive.'
source: usgs-mcs2026-bauxite-alumina
where: 'World Alumina Refinery and Bauxite Mine Production table, bauxite 2025e (world total 440,000 thousand t; shares calculated here); Recycling; Substitutes. EU list: see source ec-crm'
- subject: Alumina (aluminium oxide)
producers:
- country: China
share_percent: 62
year: 2025
- country: Australia
share_percent: 11.3
year: 2025
- country: Brazil
share_percent: 7.3
year: 2025
- country: India
share_percent: 5.5
year: 2025
- country: Russia
share_percent: 1.9
year: 2025
recycling: 'USGS bauxite and alumina chapter: ''None.'''
substitutes:
- 'USGS: other raw materials such as alunite, anorthosite, coal wastes and oil shales offer potential alumina sources.'
source: usgs-mcs2026-bauxite-alumina
where: World Alumina Refinery production table, alumina 2025e (world total 150,000 thousand t; shares calculated here); Recycling; Substitutes
- subject: Magnesium (metal)
producers:
- country: China
share_percent: 86.4
year: 2025
- country: Russia
share_percent: 5.5
year: 2025
- country: Brazil
share_percent: 1.8
year: 2025
- country: Israel
share_percent: 1.8
year: 2025
- country: Turkey
share_percent: 1.4
year: 2025
critical_lists:
- list: USGS 2025 List of Critical Minerals (listed as Magnesium)
listed: true
- list: EU list of 34 critical raw materials (Magnesium listed)
listed: true
recycling: 'USGS: in 2025 about 26,000 tons of secondary magnesium was recovered from old scrap and 82,000 tons from new scrap.'
substitutes:
- 'USGS: aluminum and zinc may substitute for magnesium in castings and wrought products; magnesium''s lower weight is an advantage, but its high cost is a disadvantage.'
source: usgs-mcs2026-magnesium-metal
where: 'World Primary Production table, smelter production 2025 (world total 1,100 thousand t; shares calculated here); Recycling; Substitutes. Lists: see sources usgs-crit2025 and ec-crm'
documents:
- title: Aluminium Alloy AA-5083 H116 Data Sheet (Dinco Trading LLC, Dubai)
type: datasheet
url: https://www.dinco.ae/files/aluminium-alloy-5083H116-data-sheet.pdf
- title: 5083 Aluminium Technical Datasheet (Smiths Metal Centres, UK; footer 2023)
type: datasheet
url: https://www.smithmetal.com/pdf/aluminium/5xxx/5083.pdf
year: 2023
- title: '5083 grade page (Alloys International): W.Nr 3.3547, EN AW-5083 / AlMg4.5Mn0.7 and specifications'
type: datasheet
url: https://alloysintl.com/inventory/aluminum-alloys/aluminum-5083/
- title: 'NIST Cryogenic Material Properties: 5083 Aluminum (UNS A95083)'
type: database
url: https://trc.nist.gov/cryogenics/materials/5083%20Aluminum/5083Aluminum_rev.htm
- title: An Extremely Low Temperature Properties of Wrought Aluminum Alloys (Kor. J. Mater. Res. 17(4), 2007; open PDF with English abstract and tables)
type: paper
url: https://koreascience.kr/article/JAKO200727542962161.pdf
year: 2007
- title: 'USGS Mineral Commodity Summaries 2026: Aluminum'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-aluminum.pdf
year: 2026
- title: 'USGS Mineral Commodity Summaries 2026: Bauxite and Alumina'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-bauxite-alumina.pdf
year: 2026
- title: 'USGS Mineral Commodity Summaries 2026: Magnesium Metal'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-magnesium-metal.pdf
year: 2026
- title: 'PubChem: Aluminum, CID 5359268, GHS classification'
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/5359268
- title: 'PubChem: Magnesium, CID 5462224, GHS classification'
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/5462224
- title: 'PubChem: Manganese, CID 23930, GHS classification'
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/23930
gaps:
- 'H321, the stabilised marine plate temper named in the request: no readable source printed values for it, so no H321 rows are recorded.'
- ASTM B209 and ASTM B928 are not printed by any source read in this run, so they are not recorded as designations.
- 'Exfoliation corrosion and stress-corrosion cracking: no source read prints a rating or test result for 5083, so neither is recorded.'
- The 65 °C caution is printed by three suppliers, but none of the sources read names sensitisation or intergranular attack as its cause.
- 'Cryogenic strength and elongation: the 2007 Korean study gives 5083 results only as figures, so no numeric cryogenic values are recorded.'
- 'Fatigue strength, fracture toughness, specific heat and Poisson''s ratio: not found in a readable source.'
- 'Space environment (vacuum outgassing, atomic oxygen, radiation, thermal cycling, flight): no source for 5083 was found in this run, so no environment tags are set.'
- The Dinco sheet, Smith Metal and AZoM print the same density, melting point, expansion, modulus and conductivity values, probably from one common supplier table, so they are not independent confirmations.
- Melting point is one printed value (570 °C). The solidus and liquidus are not printed.
- 'Electrical resistivity: AZoM prints 0.58 x 10-6 Ohm.m for the same property, ten times the Dinco value. The Dinco value (0.058 x 10-6 Ohm.m) is recorded and the AZoM value is not.'
- Titanium and zinc limits differ. The Dinco sheet prints Ti 0.05 to 0.25 and Zn 0.00 to 0.10; Smith Metal, AZoM and the 2007 paper print Ti max 0.15 and Zn max 0.25, and the Smith Metal limits are recorded. The Smith Metal composition table also has a stray 0.15 in its minimum row under Ti, so only its maxima are used.
- Hardness (Brinell and Vickers) and shear strength are not in the property list, so they are recorded as hardness_brinell, hardness_vickers and shear_strength.
- GM41 (Smith Metal, AZoM) is not recorded because the designation list has no GM system. QQ-A-250/6 (Alloys International) is not recorded for the same reason, and AMS 200/4 could not be confirmed as a 5083 specification from another source. 'AlMg4.5Mn' and 'marine aluminium' are not designations.
- Product form of AMS 4056 and MIL-A-46027 is not printed on the grade page.
- Failure-risk severity is not printed in any source read, so no severity is assigned to the two failure risks.
- No safety data sheet for 5083 was read. The hazard entries are PubChem element-level data for aluminium, magnesium and manganese; dust and fume from cutting or welding are not recorded.
- Crustal abundance of aluminium, magnesium and manganese was not looked up in this run.
- No image was fetched in this run, so the profile has no media entry.
- 'Not reached: MatWeb (asm.matweb.com) gave no response; the Clinton Aluminum cryogenic page gave no response; eFunda gave a server error; MakeItFrom returned a JavaScript and cookie check, which was not read.'
- EN AW-5083 and 3.3547 come from one supplier page (Alloys International). No second source printing them was read.
- Web search was unavailable in this run (its budget was used up). A follow-up search could find H321 data and the ASTM specifications.
sources:
dinco-5083h116:
title: Aluminium Alloy AA-5083 H116 Data Sheet (Dinco Trading LLC, Dubai)
url: https://www.dinco.ae/files/aluminium-alloy-5083H116-data-sheet.pdf
kind: datasheet
license: supplier datasheet, cited not reproduced
smith-5083-datasheet:
title: 5083 Aluminium Technical Datasheet (Smiths Metal Centres, UK; footer 2023)
url: https://www.smithmetal.com/pdf/aluminium/5xxx/5083.pdf
year: 2023
kind: datasheet
license: supplier datasheet, cited not reproduced
smith-5083-page:
title: 5083 Aluminium product page (Smiths Metal Centres, UK)
url: https://www.smithmetal.com/5083.htm
kind: web
license: supplier web page, cited not reproduced
azom-aalco-5083:
title: 'Aluminium 5083: Properties, Fabrication and Applications (AZoM article 2804; text sourced from Aalco)'
id: AZoM ArticleID 2804; page dated 2005, cited as 2020
url: https://www.azom.com/article.aspx?ArticleID=2804
year: 2020
kind: web
license: web article, cited not reproduced
alloysintl-5083:
title: '5083 grade page (Alloys International, Ronkonkoma NY): W.Nr, EN designation and specifications'
url: https://alloysintl.com/inventory/aluminum-alloys/aluminum-5083/
kind: datasheet
license: supplier web page, cited not reproduced
nist-5083:
title: 'Material Properties: 5083 Aluminum (UNS A95083), NIST Cryogenic Material Properties'
url: https://trc.nist.gov/cryogenics/materials/5083%20Aluminum/5083Aluminum_rev.htm
kind: database
license: NIST public web page
koreascience-2007:
title: An Extremely Low Temperature Properties of Wrought Aluminum Alloys (Kor. J. Mater. Res. 17(4), 2007)
id: Kor. J. Mater. Res. Vol. 17, No. 4 (2007)
url: https://koreascience.kr/article/JAKO200727542962161.pdf
year: 2007
kind: paper
license: open PDF on KoreaScience, cited not reproduced
pubchem-al:
title: 'Aluminum, PubChem CID 5359268: Safety and Hazards, GHS Classification'
url: https://pubchem.ncbi.nlm.nih.gov/compound/5359268
kind: database
license: PubChem (NCBI) public data
pubchem-mg:
title: 'Magnesium, PubChem CID 5462224: Safety and Hazards, GHS Classification'
url: https://pubchem.ncbi.nlm.nih.gov/compound/5462224
kind: database
license: PubChem (NCBI) public data
pubchem-mn:
title: 'Manganese, PubChem CID 23930: Safety and Hazards, GHS Classification'
url: https://pubchem.ncbi.nlm.nih.gov/compound/23930
kind: database
license: PubChem (NCBI) public data
usgs-mcs2026-aluminum:
title: 'Mineral Commodity Summaries 2026: Aluminum'
id: USGS MCS 2026, February 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-aluminum.pdf
year: 2026
kind: report
license: public domain (USGS)
usgs-mcs2026-bauxite-alumina:
title: 'Mineral Commodity Summaries 2026: Bauxite and Alumina'
id: USGS MCS 2026, February 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-bauxite-alumina.pdf
year: 2026
kind: report
license: public domain (USGS)
usgs-mcs2026-magnesium-metal:
title: 'Mineral Commodity Summaries 2026: Magnesium Metal'
id: USGS MCS 2026, February 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-magnesium-metal.pdf
year: 2026
kind: report
license: public domain (USGS)
usgs-crit2025:
title: About the 2025 List of Critical Minerals (USGS; the final list, posted in the Federal Register)
url: https://www.usgs.gov/programs/mineral-resources-program/science/about-2025-list-critical-minerals
year: 2025
kind: web
license: public domain (USGS)
ec-crm:
title: Critical raw materials (European Commission; fifth list of 34 critical raw materials, 2023)
url: https://single-market-economy.ec.europa.eu/sectors/raw-materials/areas-specific-interest/critical-raw-materials_en
kind: web
license: European Commission web page
license: CC-BY-4.0
updated: '2026-10-24'
review:
status: draft
method: assistant
checked_values: 22
unreachable: 0
caveats: 4
note: Written 2026-10-24 by an AI assistant from pages fetched in this run. Web search was unavailable (its budget was used up), so pages were fetched directly or by links found on fetched pages. MakeItFrom returned a JavaScript and cookie check and was not read. The O and H111 values are printed together by the sources. The AZoM electrical resistivity (0.58 x 10-6 Ohm.m) differs from the Dinco value recorded (0.058 x 10-6 Ohm.m).
story:
recipe:
line: 5083 is a wrought aluminium-magnesium alloy. The Smith Metal datasheet gives magnesium at 4.00 to 4.90 wt% and manganese at 0.40 to 1.00 wt% as the main additions, with chromium at 0.05 to 0.25 wt% and small maximum limits for iron, silicon, copper, zinc and titanium. Aluminium is the balance. The Dinco sheet places the alloy among the non-heat-treatable alloys.
parts:
- name: Aluminium
symbol: Al
share_note: balance (the rest)
role: The matrix of the alloy; the balance after the alloying limits.
source: smith-5083-datasheet
where: Chemical Composition (weight %) table, Al Bal
- name: Magnesium
symbol: Mg
share_percent: 4
share_high: 4.9
role: Main alloying element, printed range 4.00 to 4.90 wt%.
source: smith-5083-datasheet
where: Chemical Composition (weight %) table, Mg min and max
- name: Manganese
symbol: Mn
share_percent: 0.4
share_high: 1
role: Alloying addition inside the printed range; the sources read do not describe its function.
source: smith-5083-datasheet
where: Chemical Composition (weight %) table, Mn min and max
- name: Chromium
symbol: Cr
share_percent: 0.05
share_high: 0.25
role: Minor addition inside the printed range; the sources read do not describe its function.
source: smith-5083-datasheet
where: Chemical Composition (weight %) table, Cr min and max
- name: Iron
symbol: Fe
share_note: max 0.40
role: Limited to the printed maximum.
source: smith-5083-datasheet
where: Chemical Composition (weight %) table, Fe max
- name: Silicon
symbol: Si
share_note: max 0.40
role: Limited to the printed maximum.
source: smith-5083-datasheet
where: Chemical Composition (weight %) table, Si max
- name: Copper
symbol: Cu
share_note: max 0.10
role: Limited to the printed maximum.
source: smith-5083-datasheet
where: Chemical Composition (weight %) table, Cu max
- name: Zinc
symbol: Zn
share_note: max 0.25
role: Limited to the printed maximum.
source: smith-5083-datasheet
where: Chemical Composition (weight %) table, Zn max
- name: Titanium
symbol: Ti
share_note: max 0.15
role: Limited to the printed maximum (the Dinco sheet prints 0.05 to 0.25).
source: smith-5083-datasheet
where: Chemical Composition (weight %) table, Ti max
risk_groups:
- title: For people
lead: No safety data sheet for the alloy was read in this run. The hazard entries are PubChem's element-level data for aluminium, magnesium and manganese.
gap: Hazard classification for 5083 as supplied, and for dust or fume from cutting or welding, was not found in a source read in this run.
points:
- label: What the sources cover
line: The sources read describe the metals' flammability and water reactivity as classified in PubChem's company reports, and the suppliers' corrosion and welding behaviour. They do not describe health effects of the alloy.
- title: If it fails
lead: These are the failure routes named in the sources. They are supplier statements and laboratory results, not field incident data.
points:
- label: Use above 65 °C
line: The suppliers say not to use the alloy above 65 °C. The sources read do not say what happens above that limit.
- label: Long exposure to liquid nitrogen
line: In a 2007 laboratory study, the elongation of Al 5083 at cryogenic temperature fell with longer immersion in liquid nitrogen. The abstract attributes this to non-uniform fracture of precipitates on grain boundaries.
- title: Handling and welding
points:
- label: Welding
line: Arc and resistance welding are rated excellent and gas welding average. Brazing is rated poor. AZoM recommends filler 5183 for welding 5083 to itself.
- label: Machining
line: Machinability is rated poor, and cold workability average.
why: 5083 is an aluminium-magnesium alloy sold for marine and pressure-vessel work. Magnesium, at 4.00 to 4.90 wt%, is the main addition. The Dinco sheet says the alloy has the highest strength of the non-heat-treatable aluminium alloys, is highly resistant to attack by seawater and industrial chemicals, and keeps its strength after welding. The suppliers list shipbuilding, pressure vessels, vehicle bodies and rail cars as typical uses, and they advise against use above 65 °C.
uses:
- where: Ships and marine structures
line: The Dinco sheet, Smith Metal and AZoM all list shipbuilding. The Dinco sheet also lists marine applications and drilling rigs.
- where: Pressure vessels
line: All three supplier pages list pressure vessels as a typical use.
- where: Vehicle bodies, rail cars and mine skips
line: Smith Metal and AZoM list rail cars, vehicle bodies and tipper truck bodies, and both also list mine skips and cages.
- where: Research on cryogenic hydrogen tanks
line: A 2007 Korean laboratory study tested aluminium alloys, including Al 5083, for automobile hydrogen storage tanks in liquid nitrogen. It is a laboratory study, not a product record.
can_do:
- label: Strength by temper
value: Minimum proof stress 125 to 215 MPa
line: Minimum proof stress is 125 MPa for O/H111 sheet and 215 MPa for H32 sheet (BS EN 485-2 values on AZoM), and 195 MPa for H116 sheet and plate (Dinco). Tensile ranges printed are 275 to 350 MPa for O/H111 sheet, 305 to 380 MPa for H32 sheet and 305 to 385 MPa for H116.
- label: Weight
benchmark: density
line: Density is 2.65 g/cm3, as printed by Smith Metal and Dinco.
- label: Stiffness
benchmark: elastic_modulus
line: Modulus of elasticity is 72 GPa (Smith Metal).
- label: Heat conduction
benchmark: thermal_conductivity
line: Thermal conductivity is 121 W/(m·K) (Smith Metal).
- label: Welding
value: Arc and resistance welding rated excellent
line: Arc and resistance welding are rated excellent and gas welding average. The alloy keeps its strength after welding (Dinco, Smith Metal, AZoM).
- label: Seawater
value: Highly resistant
line: The suppliers rate the alloy highly resistant to attack by seawater and industrial chemicals (Dinco, Smith Metal, AZoM).
compare: 5083 is a strong, weldable, seawater-resistant option for marine structures kept at or below 65 °C. The record holds no like-for-like figures for other alloys or for space use, so this profile does not rank it against other materials.
compare_rows:
- label: Density
benchmark: density
- label: Yield strength
benchmark: yield_strength
- label: Thermal conductivity
benchmark: thermal_conductivity
handling:
- Weld 5083 to itself with filler 5183 (AZoM). Arc and resistance welding are rated excellent.
- Keep service at or below 65 °C, the limit the suppliers print.
- Machinability is rated poor (Dinco and AZoM).
good_for:
- Marine structures and ships, where the suppliers cite seawater resistance and good weldability (Dinco, Smith Metal, AZoM).
- Pressure vessels kept at or below 65 °C (Dinco, Smith Metal, AZoM).
- Rail cars and vehicle bodies, which the suppliers list as typical uses (Smith Metal, AZoM).
- 'Low-temperature service: the Smith Metal product page says the alloy performs well at low temperature. No numbers are printed.'
watch_out:
- Service above 65 °C. The suppliers say not to use the alloy there.
- Long exposure to liquid nitrogen lowered the elongation of 5083 in a 2007 laboratory study.
- Strength values come from supplier and distributor pages for O/H111, H32 and H116, and some are minimum values. H321 values, ASTM designations and space data were not found.
verdict: 5083 is a weldable marine aluminium alloy with supplier-rated seawater resistance and a 65 °C service limit. The record leaves out the H321 marine temper, the ASTM designations, exfoliation data and any space-environment data.
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.