Ethylene-vinyl acetate copolymer EVA
(C2H4)n(C4H6O2)m, a copolymer of ethylene (C2H4) and vinyl acetate (C4H6O2) as printed in the Wikipedia infobox · CAS 24937-78-8
Also known as EVA 150028, EVA 43031.CD
Ethylene-vinyl acetate copolymer (EVA) is a thermoplastic made from ethylene and vinyl acetate.
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Stiffness
19 MPa for EVA 150028
Softness
75 Shore A for EVA 150028
Stretch
522 % for EVA 150028
Melting
66 °C for EVA 150028
Recipe, share of the weight
- C2H4 balance (the rest of the weight after vinyl acetate)Ethylene
- C4H6O2 27.6 wt% in EVA 150028 and 31.4 wt% in EVA 43031.CD, per the ExxonMobil datasheetsVinyl acetate
Best for
Hot-melt adhesive, sealant and wire-compound grades in the ExxonMobil datasheets, such as EVA 150028 with a melt index of 150 g/10 min at 190 °C/2.16 kg
Weakest at
Heat and light ageing: the datasheet peak melting temperatures are 66 °C and 59 °C, and the 1983 JPL abstract reports acetic acid formation at higher temperatures
Risk at a glance
- People Low. Not classified; cancer note in SDS
- If it fails Moderate. Acetic acid release from photo-oxidation at higher temperature
- Corrosion Moderate. At higher temperatures additives leach out and evaporate, and volatile products such as acetic acid form.
Quick facts: EVA
| Property | Value | Basis |
|---|---|---|
| Density | 0.91 to 0.97 g/cm³ | 4 sourced values across conditions |
| Tensile strength | 2.3 to 4 MPa | 2 sourced values across conditions |
| Melting point | 35 to 110 °C | 4 sourced values across conditions |
What is the density of Ethylene-vinyl acetate copolymer (EVA)?
Ethylene-vinyl acetate copolymer (EVA) has a density of 0.91 to 0.97 g/cm³. The range covers 4 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the melting point of Ethylene-vinyl acetate copolymer (EVA)?
Ethylene-vinyl acetate copolymer (EVA) has a melting point of 35 to 110 °C. The range covers 4 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the tensile strength of Ethylene-vinyl acetate copolymer (EVA)?
Ethylene-vinyl acetate copolymer (EVA) has a tensile strength of 2.3 to 4 MPa. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What are the other names and codes for Ethylene-vinyl acetate copolymer (EVA)?
Ethylene-vinyl acetate copolymer (EVA) is also written as EVA 150028, EVA 43031.CD. Each code is printed in the source listed beside it in the designations table.
What is Ethylene-vinyl acetate copolymer (EVA) used for?
Uses recorded in the sources include Encapsulant for crystalline silicon solar cells in photovoltaic modules (terrestrial modules, not a space source); Wire and cable compounds, molding compounds and extrusion compounds.
Why it exists
EVA is a copolymer of ethylene and vinyl acetate, and its vinyl acetate content changes its stiffness, melting point and density. ExxonMobil's EVA 150028, with 27.6 wt% vinyl acetate, has a density of 0.945 g/cm3, a melt index of 150 g/10 min at 190 °C/2.16 kg, a Shore A hardness of 75 at 15 sec and a tensile strength at break of 2.3 MPa. Its datasheet peak melting temperature is 66 °C.
Where it's used
Solar-cell encapsulant
Wikipedia says EVA is used for crystalline silicon solar cells, where it protects the silicon and bonds it to the glass support. A 1983 JPL study tested a stabilised EVA formulation as an encapsulant for photovoltaic modules, from its abstract.
Hot-melt adhesives and sealants
The ExxonMobil EVA 150028 datasheet lists adhesives and sealants, hot melt adhesives and wax blends as its applications.
Wire, cable and molding compounds
The ExxonMobil EVA 43031.CD datasheet lists crosslinkable compounds, molding compounds, extrusion compounds and wire and cable compounds.
Closed-cell foam
Wikipedia says closed-cell EVA foam is used in play mats, sports padding and sports-shoe midsoles.
Recipe
(C2H4)n(C4H6O2)m, a copolymer of ethylene (C2H4) and vinyl acetate (C4H6O2) as printed in the Wikipedia infobox
EVA is a copolymer of ethylene and vinyl acetate. Wikipedia gives its formula as (C2H4)n(C4H6O2)m. Vinyl acetate is made from ethylene and acetic acid with oxygen over a palladium catalyst (Wikipedia).
| Ingredient | Share of the weight | What it does |
|---|---|---|
| Ethylene C2H4 | balance (the rest of the weight after vinyl acetate) | Monomer that forms the backbone. It is the balance of the copolymer after the vinyl acetate share. |
| Vinyl acetate C4H6O2 | 27.6 wt% in EVA 150028 and 31.4 wt% in EVA 43031.CD, per the ExxonMobil datasheets | Comonomer that sets the vinyl acetate content of the grade and so its stiffness, melting point and density. |
Weight shares are as printed in the sources.
What it can do
Stiffness
19 MPa for EVA 150028
measured
EVA 150028 has a flexural modulus of 19 MPa (1% secant, ExxonMobil typical value). EVA 43031.CD has 9.6 MPa.
Softness
75 Shore A for EVA 150028
measured
EVA 150028 has a Shore A hardness of 75 at 15 sec, and EVA 43031.CD has 63.
Stretch
522 % for EVA 150028
measured
EVA 150028 elongates 522 % at break. EVA 43031.CD is printed as more than 723 %.
Melting
66 °C for EVA 150028
measured
The datasheet peak melting temperatures are 66 °C for EVA 150028 and 59 °C for EVA 43031.CD. The two SDS ranges are wider, at 35 to 110 °C for the copolymer and 60 to 105 °C for the Hanwha family.
How it compares
The two ExxonMobil grades differ in vinyl acetate content (27.6 wt% against 31.4 wt%), and that gap shows in their datasheet values. EVA 43031.CD has a higher density (0.955 g/cm3 against 0.945 g/cm3), a lower peak melting temperature (59 °C against 66 °C) and a lower flexural modulus (9.6 MPa against 19 MPa). The SDS melting ranges are wider than either datasheet value, and the sources do not agree on one melting point for EVA, so both values are shown side by side. This profile does not rank EVA against other polymers, because the other profiles use different grades and test conditions.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | EVA | COC | EPDM | HDPE | PMP (TPX) | PE | PK | PP | PVC | UHMWPE |
|---|---|---|---|---|---|---|---|---|---|---|
| Thermal behavior and safety | ||||||||||
| Peak melting temperature, EVA 150028 | 66 °C4 | no data | no data | 130 to 135 °C | 232 °C | 128 °C | > 220 °C | 140 °C | no data | 135 °C |
| Peak melting temperature, EVA 43031.CD | 59 °C14 | no data | no data | 130 to 135 °C | 232 °C | 128 °C | > 220 °C | 140 °C | no data | 135 °C |
| Melting point range, Hanwha EVA grades (family SDS) | 60 to 105 °C20 | no data | no data | 130 to 135 °C | 232 °C | 128 °C | > 220 °C | 140 °C | no data | 135 °C |
| Melting point range, EVA copolymer (ExxonMobil SDS, no grade named)SDS Section 9 value, ExxonMobil in-house method | 35 to 110 °C | no data | no data | 130 to 135 °C | 232 °C | 128 °C | > 220 °C | 140 °C | no data | 135 °C |
| Physical and electrical | ||||||||||
| Density, EVA 150028 | 0.945 g/cm³1 | 1020 kg/m3 | 1.19 g/cm³ | 0.959 g/cm³ | 833 kg/m3 | 0.959 g/cm³ | 0.948 g/cm³ | 0.9 g/cm³ | 1.32 g/cc | 0.93 g/cc |
| Durometer hardness Shore A, 15 sec, EVA 150028 | 75 -9 | no data | no data | no data | no data | no data | 85 Shore A | no data | no data | no data |
| Durometer hardness Shore D, 15 sec, EVA 150028 | 19 -10 | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Density, EVA 43031.CD | 0.955 g/cm³11 | 1020 kg/m3 | 1.19 g/cm³ | 0.959 g/cm³ | 833 kg/m3 | 0.959 g/cm³ | 0.948 g/cm³ | 0.9 g/cm³ | 1.32 g/cc | 0.93 g/cc |
| Durometer hardness Shore A, 15 sec, EVA 43031.CD | 63 -18 | no data | no data | no data | no data | no data | 85 Shore A | no data | no data | no data |
| Durometer hardness Shore D, 15 sec, EVA 43031.CD | 13 -19 | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Relative density, Hanwha EVA grades (family SDS) | 0.92 to 0.95 g/cm³21 | 1020 kg/m3 | 1.19 g/cm³ | 0.959 g/cm³ | 833 kg/m3 | 0.959 g/cm³ | 0.948 g/cm³ | 0.9 g/cm³ | 1.32 g/cc | 0.93 g/cc |
| Density range, EVA copolymer (ExxonMobil SDS, no grade named)SDS Section 9 value, ExxonMobil in-house method | 0.91 to 0.97 g/cm³23 | 1020 kg/m3 | 1.19 g/cm³ | 0.959 g/cm³ | 833 kg/m3 | 0.959 g/cm³ | 0.948 g/cm³ | 0.9 g/cm³ | 1.32 g/cc | 0.93 g/cc |
| Temperature behavior | ||||||||||
| Vicat softening temperature, EVA 150028 | 51 °C5 | 133 °C | no data | 80 °C | 168 °C | no data | 49 °C | 130 °C | 79 to 81 °C | no data |
| Auto-ignition temperature, Hanwha EVA grades (family SDS)Value printed in SDS Section 9.1 | 400 °C22 | no data | no data | no data | no data | no data | > 250 °C | no data | no data | no data |
| Other measurements | ||||||||||
| Melt index, EVA 150028 | 150 g/10 min2 | no data | no data | 18 g/10 min | 26 g/10min | no data | 49 g/10 min | 12 g/10 min | no data | no data |
| Vinyl acetate content, EVA 150028 | 27.6 wt%3 | no data | no data | no data | no data | no data | 28 wt% | no data | no data | no data |
| Tensile strength at break, EVA 150028 | 2.3 MPa6 | 46 MPa | 10.5 MPa | no data | 25 MPa | 21 MPa | 19 MPa | no data | 33 MPa | 40 MPa |
| Elongation at break, EVA 150028 | 522 %7 | 120 % | 255 % | > 400 % | 22 % | 400 % | 25 % | no data | 140 % | 300 % |
| Flexural modulus, 1% secant, EVA 150028 | 19 MPa8 | no data | no data | 13000 kg/cm² | 1450 MPa | no data | 24 MPa | 1480 MPa | 2.65 GPa | 0.6 GPa |
| Melt index, EVA 43031.CD | 43 g/10 min12 | no data | no data | 18 g/10 min | 26 g/10min | no data | 49 g/10 min | 12 g/10 min | no data | no data |
| Vinyl acetate content, EVA 43031.CD | 31.4 wt%13 | no data | no data | no data | no data | no data | 28 wt% | no data | no data | no data |
| Tensile strength at break, EVA 43031.CD | > 4 MPa15 | 46 MPa | 10.5 MPa | no data | 25 MPa | 21 MPa | 19 MPa | no data | 33 MPa | 40 MPa |
| Elongation at break, EVA 43031.CD | > 723 %16 | 120 % | 255 % | > 400 % | 22 % | 400 % | 25 % | no data | 140 % | 300 % |
| Flexural modulus, 1% secant, EVA 43031.CD | 9.6 MPa17 | no data | no data | 13000 kg/cm² | 1450 MPa | no data | 24 MPa | 1480 MPa | 2.65 GPa | 0.6 GPa |
| Flash point, Hanwha EVA grades (family SDS)Value printed in SDS Section 9.1 | > 270 °C | no data | no data | no data | no data | no data | > 93 °C | no data | no data | > 662 °F |
Why choose it, and why not
Good for
- Adhesive and sealant use. EVA 150028 has a melt index of 150 g/10 min at 190 °C/2.16 kg and a peak melting temperature of 66 °C, per its datasheet.
- Flexible parts. EVA 150028 has a Shore A hardness of 75 and an elongation at break of 522 %.
- Wire and cable compounds. EVA 43031.CD is listed for these, with a melt index of 43 g/10 min.
Watch out for
- Ageing: the 1983 JPL abstract reports acetic acid among the volatile products at higher temperatures. No retention figure after UV exposure was read.
- Melting range: the datasheets give peak melting temperatures of 66 °C and 59 °C, while the SDS ranges run to 110 °C, so the value depends on the source.
- Carcinogenicity: the ExxonMobil SDS says the product 'May cause cancer', based on its vinyl acetate component.
- Acetic acid: heat and hydrolysis can form acetic acid, and the SDS lists it among thermal degradation products.
EVA is a practical, low-melting copolymer whose datasheet values for two ExxonMobil grades are well sourced, but its ageing data are thin: one 1983 abstract, and no flight, erosion or outgassing values for EVA were found in this run.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Other names and standards
The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.
| System | Codes |
|---|---|
| Trade name | EVA 150028, EVA 43031.CD |
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Density, EVA 150028 | Typical value printed on the ExxonMobil datasheet; Test Based On column reads ASTM D1505 | grade EVA 150028 (27.6 wt% vinyl acetate)test standard ASTM D1505, as printed in the Test Based On columntemperature not printed | — |
| 2 | Melt index, EVA 150028 | Typical value printed on the ExxonMobil datasheet; Test Based On column reads ASTM D1238 | grade EVA 150028temperature 190 °Cload 2.16 kg | — |
| 3 | Vinyl acetate content, EVA 150028 | Typical value printed on the ExxonMobil datasheet; method column reads ExxonMobil Method | grade EVA 150028 | Custom name, not in the canonical property list |
| 4 | Peak melting temperature, EVA 150028 | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method | grade EVA 150028english unit as printed 151 °F | — |
| 5 | Vicat softening temperature, EVA 150028 | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method, test standard not printed | grade EVA 150028english unit as printed 124 °F | — |
| 6 | Tensile strength at break, EVA 150028 | Typical value printed on the ExxonMobil datasheet; the datasheet states that all physical properties were measured on compression molded specimens | grade EVA 150028specimen compression moldedenglish unit as printed 330 psi | — |
| 7 | Elongation at break, EVA 150028 | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method | grade EVA 150028specimen compression molded | — |
| 8 | Flexural modulus, 1% secant, EVA 150028 | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method | grade EVA 150028secant 1% secantenglish unit as printed 2700 psi | — |
| 9 | Durometer hardness Shore A, 15 sec, EVA 150028 | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method | grade EVA 150028duration 15 sec | Custom name. Shore hardness is a scale with no unit, recorded as - |
| 10 | Durometer hardness Shore D, 15 sec, EVA 150028 | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method | grade EVA 150028duration 15 sec | Custom name. Shore hardness is a scale with no unit, recorded as - |
| 11 | Density, EVA 43031.CD | Typical value printed on the ExxonMobil datasheet; Test Based On column reads ASTM D1505 | grade EVA 43031.CD (31.4 wt% vinyl acetate)test standard ASTM D1505, as printed in the Test Based On columntemperature not printed | — |
| 12 | Melt index, EVA 43031.CD | Typical value printed on the ExxonMobil datasheet; Test Based On column reads ASTM D1238 | grade EVA 43031.CDtemperature 190 °Cload 2.16 kg | — |
| 13 | Vinyl acetate content, EVA 43031.CD | Typical value printed on the ExxonMobil datasheet; method column reads ExxonMobil Method | grade EVA 43031.CD | Custom name, not in the canonical property list |
| 14 | Peak melting temperature, EVA 43031.CD | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method | grade EVA 43031.CDenglish unit as printed 138 °F | — |
| 15 | Tensile strength at break, EVA 43031.CD | Typical value printed on the ExxonMobil datasheet; the datasheet states that all physical properties were measured on compression molded specimens | grade EVA 43031.CDspecimen compression moldedbound as printed > 4.0 MPa (> 580 psi) | — |
| 16 | Elongation at break, EVA 43031.CD | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method | grade EVA 43031.CDspecimen compression moldedbound as printed > 723 % | — |
| 17 | Flexural modulus, 1% secant, EVA 43031.CD | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method | grade EVA 43031.CDsecant 1% secantenglish unit as printed 1400 psi | — |
| 18 | Durometer hardness Shore A, 15 sec, EVA 43031.CD | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method | grade EVA 43031.CDduration 15 sec | Custom name. Shore hardness is a scale with no unit, recorded as - |
| 19 | Durometer hardness Shore D, 15 sec, EVA 43031.CD | Typical value printed on the ExxonMobil datasheet; ExxonMobil Method | grade EVA 43031.CDduration 15 sec | Custom name. Shore hardness is a scale with no unit, recorded as - |
| 20 | Melting point range, Hanwha EVA grades (family SDS) | Value printed in SDS Section 9.1 and marked in the SDS as typical values | basis Hanwha EVA family SDS covering the grades listed in Section 1.1.1, not one gradeprinted 60℃~105℃ | — |
| 21 | Relative density, Hanwha EVA grades (family SDS) | Value printed in SDS Section 9.1 and marked in the SDS as typical values | basis Hanwha EVA family SDS covering the grades listed in Section 1.1.1, not one gradetemperature 25 ℃printed 0.92~0.95g/cm3(25℃) | — |
| 22 | Auto-ignition temperature, Hanwha EVA grades (family SDS) | — | basis Hanwha EVA family SDS covering the grades listed in Section 1.1.1, not one gradeprinted 400℃ | Custom name, not in the canonical property list |
| 23 | Density range, EVA copolymer (ExxonMobil SDS, no grade named) | — | basis ExxonMobil SDS for the Ethylene Vinyl Acetate Copolymer, with no grade namedtemperature 15 °C (59 °F)printed 0.91 to 0.97 g/cm³ [15°C (59°F)] [In-house method] | — |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Photo-oxidation in air under UV-containing light at 25 °C | low | A stabilised EVA slowly photo-oxidizes at 25 °C, and the abstract reports no change in bulk properties for up to 1500 hours.1 |
| Higher temperature in air, with additives present | moderate | At higher temperatures additives leach out and evaporate, and volatile products such as acetic acid form.2 |
| Hydrolysis | not rated | Wikipedia says hydrolysis of EVA gives ethylene vinyl alcohol copolymer and acetic acid.3 |
| Thermal processing and elevated temperature | not rated | The ExxonMobil SDS says thermal degradation products, including acetic acid, may evolve at elevated temperatures.4 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Photo-oxidation in air under UV-containing light at 25 °C | The 1983 JPL abstract says the stabilised EVA slowly photooxidized at 25 °C through energy transfer from its UV absorber, and that its bulk physical properties showed no change for up to 1500 hours of irradiation. | basis laboratory abstract of a stabilised EVA formulation; no retention figure in the abstractrating basis assigned by the assistant from the abstract wording |
| 2 | Higher temperature in air, with additives present | The 1983 JPL abstract says that at higher temperatures additives leached out and evaporated, which led to chemical crosslinking and volatile photoproducts such as acetic acid. The temperature range tested is printed as 25-105 C. | range tested 25-105 C, as printedbasis laboratory abstract, three oxygen conditions |
| 3 | Hydrolysis | Wikipedia says that hydrolysis of EVA produces the ethylene vinyl alcohol copolymer (EVOH) and acetic acid. The article gives no test conditions or rate. | basis general statement in an encyclopedia article; no test condition |
| 4 | Thermal processing and elevated temperature | The ExxonMobil SDS says that during thermal processing, aldehydes such as formaldehyde and acetaldehyde, and organic acids such as formic acid and acetic acid, may evolve at elevated temperatures. Section 10 advises avoiding elevated temperatures for prolonged periods of time. | basis SDS statement on rotomolding and processing; no test data |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
The Hanwha and ExxonMobil SDSs do not classify EVA as hazardous, but the ExxonMobil SDS gives a carcinogenicity conclusion based on its vinyl acetate component.
- Classification
- ExxonMobil classifies the copolymer as Not classified and adds the supplemental label element EUH210. Hanwha lists it as not classified for physical, health and environmental hazards.
- Vinyl acetate
- The ExxonMobil SDS lists vinyl acetate at ≥0.1 - <1 % by weight and says the product 'May cause cancer', based on the components.
- Dust
- The ExxonMobil SDS warns that fine particles can form an explosible dust-air mixture.
If it overheats
Heat and light change EVA's chemistry, and the sources name acetic acid as a product.
- Heat
- The ExxonMobil SDS says thermal degradation products such as formaldehyde, acetaldehyde, formic acid and acetic acid may evolve at elevated temperatures during processing.
- Light
- The 1983 JPL abstract reports slow photo-oxidation at 25 °C and volatile photoproducts such as acetic acid at higher temperatures.
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Acetic acid release from photo-oxidation at higher temperaturemoderate severity | UV light and heat on an EVA containing additives, as tested in the 1983 JPL studyAdditives leach out and evaporate, which led to chemical crosslinking and volatile photoproducts such as acetic acid in the study |
| Dust-air explosion when fine particles are madelow severity | Further processing, handling or grinding that generates small particles of the copolymerMay form explosible dust-air mixture, per the ExxonMobil SDS |
Handling and storage
- Avoid dust generation. The ExxonMobil SDS says to vacuum dust with equipment fitted with a HEPA filter and not to dry sweep.
- Hot material can cause thermal burns, so wear protective equipment and cool molten material with cold water, per the ExxonMobil SDS.
- Keep away from heat, sparks and flames (Hanwha SDS), and away from strong oxidizing agents, amines (Hanwha SDS) and fluorine (ExxonMobil SDS).
Mitigations
- Use local exhaust ventilation or other engineering controls where dust, fumes or vapour form, per the ExxonMobil SDS.
Supply and geography
How common the raw materials are and where they come from.
Ethylene (monomer)
Wikipedia gives worldwide ethylene production as over 225 million tonnes in 2022 and says steam cracking is a primary method.
Vinyl acetate (comonomer)
Wikipedia says vinyl acetate is made from ethylene and acetic acid with oxygen over a palladium catalyst, and that About 80% of vinyl acetate is polymerized, with ethylene-vinyl acetate among the polymers made from it.
Ethylene-vinyl acetate copolymer (manufacturer named in the Hanwha SDS)
- Top producers
- South Korea
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: eva
spore_version: 0.2
family: polyolefins
name: Ethylene-vinyl acetate copolymer
abbreviation: EVA
role: thermoplastic copolymer for solar encapsulants, hot-melt adhesives and wire compounds
category: polymers
type: polyolefins
summary: Ethylene-vinyl acetate copolymer (EVA) is a thermoplastic made from ethylene and vinyl acetate. Two ExxonMobil grades read for this profile have a density of 0.945 g/cm3 (EVA 150028, 27.6 wt% vinyl acetate) and 0.955 g/cm3 (EVA 43031.CD, 31.4 wt% vinyl acetate), with melt indexes of 150 g/10 min and 43 g/10 min at 190 °C/2.16 kg. A 1983 Jet Propulsion Laboratory abstract reports that a stabilised EVA slowly photo-oxidizes at 25 °C and forms volatile products such as acetic acid at higher temperatures.
best_for: Hot-melt adhesive, sealant and wire-compound grades in the ExxonMobil datasheets, such as EVA 150028 with a melt index of 150 g/10 min at 190 °C/2.16 kg
weakest_at: 'Heat and light ageing: the datasheet peak melting temperatures are 66 °C and 59 °C, and the 1983 JPL abstract reports acetic acid formation at higher temperatures'
identity:
formula: (C2H4)n(C4H6O2)m, a copolymer of ethylene (C2H4) and vinyl acetate (C4H6O2) as printed in the Wikipedia infobox
cas: 24937-78-8
source: wikipedia-eva
where: Infobox formula. CAS number from the Hanwha SDS, Section 3 (Ethylene Vinyl Acetate Copolymer, 24937-78-8)
designations:
- system: Trade name
code: EVA 150028
note: ExxonMobil grade name, printed as ExxonMobil EVA 150028 on the datasheet
source: exxon-150028
where: Title block and product name
- system: Trade name
code: EVA 43031.CD
note: ExxonMobil grade name, printed as ExxonMobil EVA 43031.CD on the datasheet
source: exxon-43031cd
where: Title block and product name
tags:
environments: []
stresses:
- uv
- extreme-heat
applications:
- solar-arrays
- electronics-and-chips
properties:
- benchmark: density
label: Density, EVA 150028
value: 0.945
unit: g/cm3
scope: material
conditions:
grade: EVA 150028 (27.6 wt% vinyl acetate)
test_standard: ASTM D1505, as printed in the Test Based On column
temperature: not printed
method: Typical value printed on the ExxonMobil datasheet; Test Based On column reads ASTM D1505
status: ground
source: exxon-150028
where: Resin Properties table, Density row
- benchmark: melt_flow_rate
label: Melt index, EVA 150028
value: 150
unit: g/10 min
scope: material
conditions:
grade: EVA 150028
temperature: 190 °C
load: 2.16 kg
method: Typical value printed on the ExxonMobil datasheet; Test Based On column reads ASTM D1238
status: ground
source: exxon-150028
where: Resin Properties table, Melt Index (190°C/2.16 kg) row
- benchmark: vinyl_acetate_content
label: Vinyl acetate content, EVA 150028
value: 27.6
unit: wt%
scope: material
conditions:
grade: EVA 150028
method: Typical value printed on the ExxonMobil datasheet; method column reads ExxonMobil Method
status: ground
note: Custom name, not in the canonical property list
source: exxon-150028
where: Resin Properties table, Vinyl Acetate Content row
- benchmark: melting_point
label: Peak melting temperature, EVA 150028
value: 66
unit: °C
scope: material
conditions:
grade: EVA 150028
english_unit_as_printed: 151 °F
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method
status: ground
source: exxon-150028
where: Resin Properties table, Peak Melting Temperature row
- benchmark: vicat_softening_temperature
label: Vicat softening temperature, EVA 150028
value: 51
unit: °C
scope: material
conditions:
grade: EVA 150028
english_unit_as_printed: 124 °F
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method, test standard not printed
status: ground
source: exxon-150028
where: Thermal table, Vicat Softening Temperature row
- benchmark: ultimate_tensile_strength
label: Tensile strength at break, EVA 150028
value: 2.3
unit: MPa
scope: material
conditions:
grade: EVA 150028
specimen: compression molded
english_unit_as_printed: 330 psi
method: Typical value printed on the ExxonMobil datasheet; the datasheet states that all physical properties were measured on compression molded specimens
status: ground
source: exxon-150028
where: Molded Properties table, Tensile Strength at Break row
- benchmark: elongation
label: Elongation at break, EVA 150028
value: 522
unit: '%'
scope: material
conditions:
grade: EVA 150028
specimen: compression molded
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method
status: ground
source: exxon-150028
where: Molded Properties table, Elongation at Break row
- benchmark: flexural_modulus
label: Flexural modulus, 1% secant, EVA 150028
value: 19
unit: MPa
scope: material
conditions:
grade: EVA 150028
secant: 1% secant
english_unit_as_printed: 2700 psi
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method
status: ground
source: exxon-150028
where: Molded Properties table, Flexural Modulus - 1% Secant row
- benchmark: shore_a_hardness
label: Durometer hardness Shore A, 15 sec, EVA 150028
value: 75
unit: '-'
scope: material
conditions:
grade: EVA 150028
duration: 15 sec
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method
status: ground
note: Custom name. Shore hardness is a scale with no unit, recorded as -
source: exxon-150028
where: Molded Properties table, Durometer Hardness Shore A 15 sec row
- benchmark: shore_d_hardness
label: Durometer hardness Shore D, 15 sec, EVA 150028
value: 19
unit: '-'
scope: material
conditions:
grade: EVA 150028
duration: 15 sec
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method
status: ground
note: Custom name. Shore hardness is a scale with no unit, recorded as -
source: exxon-150028
where: Molded Properties table, Durometer Hardness Shore D 15 sec row
- benchmark: density
label: Density, EVA 43031.CD
value: 0.955
unit: g/cm3
scope: material
conditions:
grade: EVA 43031.CD (31.4 wt% vinyl acetate)
test_standard: ASTM D1505, as printed in the Test Based On column
temperature: not printed
method: Typical value printed on the ExxonMobil datasheet; Test Based On column reads ASTM D1505
status: ground
source: exxon-43031cd
where: Resin Properties table, Density row
- benchmark: melt_flow_rate
label: Melt index, EVA 43031.CD
value: 43
unit: g/10 min
scope: material
conditions:
grade: EVA 43031.CD
temperature: 190 °C
load: 2.16 kg
method: Typical value printed on the ExxonMobil datasheet; Test Based On column reads ASTM D1238
status: ground
source: exxon-43031cd
where: Resin Properties table, Melt Index (190°C/2.16 kg) row
- benchmark: vinyl_acetate_content
label: Vinyl acetate content, EVA 43031.CD
value: 31.4
unit: wt%
scope: material
conditions:
grade: EVA 43031.CD
method: Typical value printed on the ExxonMobil datasheet; method column reads ExxonMobil Method
status: ground
note: Custom name, not in the canonical property list
source: exxon-43031cd
where: Resin Properties table, Vinyl Acetate Content row
- benchmark: melting_point
label: Peak melting temperature, EVA 43031.CD
value: 59
unit: °C
scope: material
conditions:
grade: EVA 43031.CD
english_unit_as_printed: 138 °F
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method
status: ground
source: exxon-43031cd
where: Resin Properties table, Peak Melting Temperature row
- benchmark: ultimate_tensile_strength
label: Tensile strength at break, EVA 43031.CD
value: 4
bound: lower
unit: MPa
scope: material
conditions:
grade: EVA 43031.CD
specimen: compression molded
bound_as_printed: '> 4.0 MPa (> 580 psi)'
method: Typical value printed on the ExxonMobil datasheet; the datasheet states that all physical properties were measured on compression molded specimens
status: ground
source: exxon-43031cd
where: Molded Properties table, Tensile Strength at Break row
- benchmark: elongation
label: Elongation at break, EVA 43031.CD
value: 723
bound: lower
unit: '%'
scope: material
conditions:
grade: EVA 43031.CD
specimen: compression molded
bound_as_printed: '> 723 %'
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method
status: ground
source: exxon-43031cd
where: Molded Properties table, Elongation at Break row
- benchmark: flexural_modulus
label: Flexural modulus, 1% secant, EVA 43031.CD
value: 9.6
unit: MPa
scope: material
conditions:
grade: EVA 43031.CD
secant: 1% secant
english_unit_as_printed: 1400 psi
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method
status: ground
source: exxon-43031cd
where: Molded Properties table, Flexural Modulus - 1% Secant row
- benchmark: shore_a_hardness
label: Durometer hardness Shore A, 15 sec, EVA 43031.CD
value: 63
unit: '-'
scope: material
conditions:
grade: EVA 43031.CD
duration: 15 sec
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method
status: ground
note: Custom name. Shore hardness is a scale with no unit, recorded as -
source: exxon-43031cd
where: Molded Properties table, Durometer Hardness Shore A 15 sec row
- benchmark: shore_d_hardness
label: Durometer hardness Shore D, 15 sec, EVA 43031.CD
value: 13
unit: '-'
scope: material
conditions:
grade: EVA 43031.CD
duration: 15 sec
method: Typical value printed on the ExxonMobil datasheet; ExxonMobil Method
status: ground
note: Custom name. Shore hardness is a scale with no unit, recorded as -
source: exxon-43031cd
where: Molded Properties table, Durometer Hardness Shore D 15 sec row
- benchmark: melting_point
label: Melting point range, Hanwha EVA grades (family SDS)
value: 60
value_high: 105
bound: range
unit: °C
scope: material
conditions:
basis: Hanwha EVA family SDS covering the grades listed in Section 1.1.1, not one grade
printed: 60℃~105℃
method: Value printed in SDS Section 9.1 and marked in the SDS as typical values
status: ground
source: hanwha-eva-sds
where: Section 9.1, Melting point/freezing point row
- benchmark: density
label: Relative density, Hanwha EVA grades (family SDS)
value: 0.92
value_high: 0.95
bound: range
unit: g/cm3
scope: material
conditions:
basis: Hanwha EVA family SDS covering the grades listed in Section 1.1.1, not one grade
temperature: 25 ℃
printed: 0.92~0.95g/cm3(25℃)
method: Value printed in SDS Section 9.1 and marked in the SDS as typical values
status: ground
source: hanwha-eva-sds
where: Section 9.1, Relative density row
- benchmark: flash_point
label: Flash point, Hanwha EVA grades (family SDS)
value: 270
bound: lower
unit: °C
scope: material
conditions:
basis: Hanwha EVA family SDS covering the grades listed in Section 1.1.1, not one grade
printed: '>270 ℃'
method: Value printed in SDS Section 9.1
status: ground
source: hanwha-eva-sds
where: Section 9.1, Flash point row
- benchmark: autoignition_temperature
label: Auto-ignition temperature, Hanwha EVA grades (family SDS)
value: 400
unit: °C
scope: material
conditions:
basis: Hanwha EVA family SDS covering the grades listed in Section 1.1.1, not one grade
printed: 400℃
method: Value printed in SDS Section 9.1
status: ground
note: Custom name, not in the canonical property list
source: hanwha-eva-sds
where: Section 9.1, Auto-ignition temperature row
- benchmark: melting_point
label: Melting point range, EVA copolymer (ExxonMobil SDS, no grade named)
value: 35
value_high: 110
bound: range
unit: °C
scope: material
conditions:
basis: ExxonMobil SDS for the Ethylene Vinyl Acetate Copolymer, with no grade named
printed: 35 to 110°C (95 to 230°F) [In-house method]
method: SDS Section 9 value, ExxonMobil in-house method
status: ground
source: exxon-eva-sds
where: Section 9, Melting point/freezing point row
- benchmark: density
label: Density range, EVA copolymer (ExxonMobil SDS, no grade named)
value: 0.91
value_high: 0.97
bound: range
unit: g/cm3
scope: material
conditions:
basis: ExxonMobil SDS for the Ethylene Vinyl Acetate Copolymer, with no grade named
temperature: 15 °C (59 °F)
printed: 0.91 to 0.97 g/cm³ [15°C (59°F)] [In-house method]
method: SDS Section 9 value, ExxonMobil in-house method
status: ground
source: exxon-eva-sds
where: Section 9, Density row
corrosion:
- environment: Photo-oxidation in air under UV-containing light at 25 °C
headline: A stabilised EVA slowly photo-oxidizes at 25 °C, and the abstract reports no change in bulk properties for up to 1500 hours.
effect: The 1983 JPL abstract says the stabilised EVA slowly photooxidized at 25 °C through energy transfer from its UV absorber, and that its bulk physical properties showed no change for up to 1500 hours of irradiation.
rating: low
conditions:
basis: laboratory abstract of a stabilised EVA formulation; no retention figure in the abstract
rating_basis: assigned by the assistant from the abstract wording
source: jpl-1983-photothermal
where: Abstract
- environment: Higher temperature in air, with additives present
headline: At higher temperatures additives leach out and evaporate, and volatile products such as acetic acid form.
effect: The 1983 JPL abstract says that at higher temperatures additives leached out and evaporated, which led to chemical crosslinking and volatile photoproducts such as acetic acid. The temperature range tested is printed as 25-105 C.
rating: moderate
conditions:
range_tested: 25-105 C, as printed
basis: laboratory abstract, three oxygen conditions
source: jpl-1983-photothermal
where: Abstract
- environment: Hydrolysis
headline: Wikipedia says hydrolysis of EVA gives ethylene vinyl alcohol copolymer and acetic acid.
effect: Wikipedia says that hydrolysis of EVA produces the ethylene vinyl alcohol copolymer (EVOH) and acetic acid. The article gives no test conditions or rate.
rating: unknown
conditions:
basis: general statement in an encyclopedia article; no test condition
source: wikipedia-eva
where: Article text on hydrolysis
- environment: Thermal processing and elevated temperature
headline: The ExxonMobil SDS says thermal degradation products, including acetic acid, may evolve at elevated temperatures.
effect: The ExxonMobil SDS says that during thermal processing, aldehydes such as formaldehyde and acetaldehyde, and organic acids such as formic acid and acetic acid, may evolve at elevated temperatures. Section 10 advises avoiding elevated temperatures for prolonged periods of time.
rating: unknown
conditions:
basis: SDS statement on rotomolding and processing; no test data
source: exxon-eva-sds
where: Section 8, Special precautions; Section 10, Conditions to avoid
risks:
hazards:
- text: ExxonMobil classifies the EVA copolymer as Not classified, with supplemental label element EUH210 (safety data sheet available on request), and reports no specific fire or explosion hazard.
ghs: []
source: exxon-eva-sds
where: Sections 2 and 5
- text: Hanwha Solutions classifies its EVA as not classified for physical, health or environmental hazards under the OSHA Hazard Communication Standard, with no pictogram or signal word.
ghs: []
source: hanwha-eva-sds
where: Sections 2.1 and 2.2
- text: The ExxonMobil SDS lists vinyl acetate (CAS 108-05-4) at ≥0.1 - <1 % by weight and gives the carcinogenicity conclusion as 'May cause cancer', based on assessment of the components.
ghs: []
source: exxon-eva-sds
where: Section 3 (ingredient table) and Section 11 (Carcinogenicity)
failure_risks:
- mode: Acetic acid release from photo-oxidation at higher temperature
trigger: UV light and heat on an EVA containing additives, as tested in the 1983 JPL study
consequence: Additives leach out and evaporate, which led to chemical crosslinking and volatile photoproducts such as acetic acid in the study
severity: moderate
source: jpl-1983-photothermal
where: Abstract
- mode: Dust-air explosion when fine particles are made
trigger: Further processing, handling or grinding that generates small particles of the copolymer
consequence: May form explosible dust-air mixture, per the ExxonMobil SDS
severity: low
source: exxon-eva-sds
where: Section 2, Other hazards which do not result in classification
side_effects: []
handling:
- text: Avoid dust generation. The ExxonMobil SDS says to vacuum dust with equipment fitted with a HEPA filter and not to dry sweep.
source: exxon-eva-sds
where: Section 6, Small spill and Large spill rows
- text: Hot material can cause thermal burns, so wear protective equipment and cool molten material with cold water, per the ExxonMobil SDS.
source: exxon-eva-sds
where: Section 4 (skin contact) and Section 7 (protective measures)
- text: Keep away from heat, sparks and flames (Hanwha SDS), and away from strong oxidizing agents, amines (Hanwha SDS) and fluorine (ExxonMobil SDS).
source: hanwha-eva-sds
where: Sections 7.2, 10.2 and 10.3
mitigations:
- text: Use local exhaust ventilation or other engineering controls where dust, fumes or vapour form, per the ExxonMobil SDS.
source: exxon-eva-sds
where: Section 8, Appropriate engineering controls
uses:
- application: solar-arrays
device: Encapsulant for crystalline silicon solar cells in photovoltaic modules (terrestrial modules, not a space source)
example: Wikipedia says EVA is used for crystalline silicon solar cells, where it protects the silicon and bonds it to the glass support.
source: wikipedia-eva
where: Uses section, Solar encapsulant
- application: electronics-and-chips
device: Wire and cable compounds, molding compounds and extrusion compounds
example: ExxonMobil EVA 43031.CD is listed for crosslinkable compounds, molding compounds, extrusion compounds and wire and cable compounds.
source: exxon-43031cd
where: General table, Applications row
supply:
- subject: Ethylene (monomer)
abundance: Wikipedia gives worldwide ethylene production as over 225 million tonnes in 2022 and says steam cracking is a primary method.
producers: []
critical_lists: []
substitutes: []
source: wikipedia-ethylene
where: Production section
- subject: Vinyl acetate (comonomer)
abundance: Wikipedia says vinyl acetate is made from ethylene and acetic acid with oxygen over a palladium catalyst, and that About 80% of vinyl acetate is polymerized, with ethylene-vinyl acetate among the polymers made from it.
producers: []
critical_lists: []
substitutes: []
source: wikipedia-vinyl-acetate
where: Production and Main use sections
- subject: Ethylene-vinyl acetate copolymer (manufacturer named in the Hanwha SDS)
producers:
- country: South Korea
critical_lists: []
substitutes: []
source: hanwha-eva-sds
where: Section 1.3.1, manufacturer address (Ulsan and Yeosu plants)
documents:
- title: ExxonMobil EVA 150028 product datasheet, effective 06/11/2020
type: datasheet
url: https://www.exxonmobilchemical.com/en/chemicals/webapi/dps/v1/datasheets/150000000456/0/en
year: 2020
- title: ExxonMobil EVA 43031.CD product datasheet, effective 06/11/2020
type: datasheet
url: https://www.exxonmobilchemical.com/en/chemicals/webapi/dps/v1/datasheets/150000000132/0/en
year: 2020
- title: ExxonMobil safety data sheet, Ethylene Vinyl Acetate Copolymer, version 8.03
type: sds
url: https://www.exxonmobilchemical.com/en/chemicals/webapi/dps/v1/safetydatasheets/1169082/en
year: 2026
- title: Hanwha Solutions safety data sheet, EVA, version 2, printed January 5, 2024
type: sds
url: https://hcc.hanwha.co.kr/static/en/data/product/msds/20240724/US_SDS_EVA_Ver.2.pdf
year: 2024
- title: Liang et al., Photothermal degradation of ethylene/vinylacetate copolymer, Jet Propulsion Laboratory, 1983 (NASA NTRS 19830065499)
type: paper
url: https://ntrs.nasa.gov/citations/19830065499
year: 1983
gaps:
- 'No atomic oxygen erosion yield for EVA: the NASA TM-2008-215490 Table I (MISSE 2 PEACE polymers) has no EVA row; it lists polypropylene and polyethylene, so no EVA erosion value is recorded.'
- No flight, vacuum outgassing, radiation or thermal-cycling result for EVA was found in the sources read in this run.
- The PubChem record for CAS 24937-78-8 returned a verification page and could not be read, so no PubChem GHS entry is recorded.
- The ExxonMobil datasheets and the ExxonMobil SDS returned Access Denied or binary PDF to direct fetches; their values were read from saved PDF copies of the same pages in this run, so a live-page check may not match them.
- Molecular weight of 700 to 50000 is printed in the ExxonMobil SDS without a unit, so it is not recorded.
- Vinyl acetate monomer values (LD50, LC50, flash point, classification) belong to the monomer, not to EVA, and are not recorded as EVA values.
- 'Glass transition: Wikipedia gives a family-level value without a grade, so no glass transition is recorded for either grade.'
- Chemical resistance (solvents, acids, bases) and retention of tensile or elongation after UV or heat exposure were not found in the sources read.
- The NREL and OSTI reports on EVA encapsulant yellowing and acetic acid could not be opened (access denied), so they are not cited.
- No producer shares or tonnages for EVA were found; the Hanwha SDS names a Korean manufacturer without a share.
- No USGS or EU critical-minerals entry was checked for EVA feedstocks.
- Shore hardness, vinyl acetate content and auto-ignition temperature are not in the canonical property list and use custom names.
- The 1 to 4 g/cm3 bulk density in the ExxonMobil SDS is a pellet bulk property, not a material density, and is not recorded.
sources:
wikipedia-eva:
title: Ethylene-vinyl acetate, Wikipedia
id: 'Article: composition, uses, hydrolysis'
url: https://en.wikipedia.org/wiki/Ethylene-vinyl_acetate
kind: web
license: CC BY-SA 4.0 (linked, not reproduced)
exxon-150028:
title: ExxonMobil EVA 150028, Ethylene Vinyl Acetate Copolymer, product datasheet
id: Effective date 06/11/2020, typical properties
url: https://www.exxonmobilchemical.com/en/chemicals/webapi/dps/v1/datasheets/150000000456/0/en
year: 2020
kind: datasheet
license: manufacturer datasheet, linked not reproduced
exxon-43031cd:
title: ExxonMobil EVA 43031.CD, Ethylene Vinyl Acetate Copolymer, product datasheet
id: Effective date 06/11/2020, typical properties
url: https://www.exxonmobilchemical.com/en/chemicals/webapi/dps/v1/datasheets/150000000132/0/en
year: 2020
kind: datasheet
license: manufacturer datasheet, linked not reproduced
hanwha-eva-sds:
title: Hanwha Solutions safety data sheet, EVA family, version 2
id: Printed January 5, 2024; OSHA HCS 29 CFR 1910.1200; CAS 24937-78-8
url: https://hcc.hanwha.co.kr/static/en/data/product/msds/20240724/US_SDS_EVA_Ver.2.pdf
year: 2024
kind: datasheet
license: supplier SDS, linked not reproduced
exxon-eva-sds:
title: ExxonMobil safety data sheet, Ethylene Vinyl Acetate Copolymer, version 8.03
id: Date of issue 13 August 2026 as printed; Section 9 in-house method values
url: https://www.exxonmobilchemical.com/en/chemicals/webapi/dps/v1/safetydatasheets/1169082/en
year: 2026
kind: datasheet
license: supplier SDS, linked not reproduced
jpl-1983-photothermal:
title: Photothermal degradation of ethylene/vinylacetate copolymer (Liang et al., Jet Propulsion Laboratory)
id: NASA accession 83A46717; abstract only
url: https://ntrs.nasa.gov/citations/19830065499
year: 1983
kind: paper
license: NASA public document
wikipedia-ethylene:
title: Ethylene, Wikipedia
id: 'Article: production and uses sections'
url: https://en.wikipedia.org/wiki/Ethylene
kind: web
license: CC BY-SA 4.0 (linked, not reproduced)
wikipedia-vinyl-acetate:
title: Vinyl acetate, Wikipedia
id: 'Article: production and main use sections'
url: https://en.wikipedia.org/wiki/Vinyl_acetate
kind: web
license: CC BY-SA 4.0 (linked, not reproduced)
license: CC-BY-4.0
updated: '2026-11-02'
review:
status: draft
method: assistant
checked_values: 25
unreachable: 0
caveats: 4
note: 'Read by an AI assistant on 2026-11-02 from the pages named in each entry. The two ExxonMobil datasheets and the ExxonMobil SDS returned Access Denied or binary PDF to direct fetches, so their text was taken from saved PDF copies of the same pages. Caveats: the Hanwha values are for a family of grades, the two SDS ranges are for the EVA copolymer with no grade named, the Shore hardness unit is -, and the ExxonMobil SDS melting and density values are in-house method.'
story:
recipe:
line: EVA is a copolymer of ethylene and vinyl acetate. Wikipedia gives its formula as (C2H4)n(C4H6O2)m. Vinyl acetate is made from ethylene and acetic acid with oxygen over a palladium catalyst (Wikipedia).
parts:
- name: Ethylene
symbol: C2H4
role: Monomer that forms the backbone. It is the balance of the copolymer after the vinyl acetate share.
share_note: balance (the rest of the weight after vinyl acetate)
source: wikipedia-eva
where: Infobox formula
- name: Vinyl acetate
symbol: C4H6O2
role: Comonomer that sets the vinyl acetate content of the grade and so its stiffness, melting point and density.
share_note: 27.6 wt% in EVA 150028 and 31.4 wt% in EVA 43031.CD, per the ExxonMobil datasheets
source: exxon-150028
where: Resin Properties table, Vinyl Acetate Content row
risk_groups:
- title: For people
lead: The Hanwha and ExxonMobil SDSs do not classify EVA as hazardous, but the ExxonMobil SDS gives a carcinogenicity conclusion based on its vinyl acetate component.
level: 1
verdict: Not classified; cancer note in SDS
points:
- label: Classification
line: ExxonMobil classifies the copolymer as Not classified and adds the supplemental label element EUH210. Hanwha lists it as not classified for physical, health and environmental hazards.
- label: Vinyl acetate
line: The ExxonMobil SDS lists vinyl acetate at ≥0.1 - <1 % by weight and says the product 'May cause cancer', based on the components.
- label: Dust
line: The ExxonMobil SDS warns that fine particles can form an explosible dust-air mixture.
- title: If it overheats
lead: Heat and light change EVA's chemistry, and the sources name acetic acid as a product.
level: 2
verdict: Acetic acid is the named by-product
points:
- label: Heat
line: The ExxonMobil SDS says thermal degradation products such as formaldehyde, acetaldehyde, formic acid and acetic acid may evolve at elevated temperatures during processing.
- label: Light
line: The 1983 JPL abstract reports slow photo-oxidation at 25 °C and volatile photoproducts such as acetic acid at higher temperatures.
why: EVA is a copolymer of ethylene and vinyl acetate, and its vinyl acetate content changes its stiffness, melting point and density. ExxonMobil's EVA 150028, with 27.6 wt% vinyl acetate, has a density of 0.945 g/cm3, a melt index of 150 g/10 min at 190 °C/2.16 kg, a Shore A hardness of 75 at 15 sec and a tensile strength at break of 2.3 MPa. Its datasheet peak melting temperature is 66 °C.
uses:
- where: Solar-cell encapsulant
line: Wikipedia says EVA is used for crystalline silicon solar cells, where it protects the silicon and bonds it to the glass support. A 1983 JPL study tested a stabilised EVA formulation as an encapsulant for photovoltaic modules, from its abstract.
- where: Hot-melt adhesives and sealants
line: The ExxonMobil EVA 150028 datasheet lists adhesives and sealants, hot melt adhesives and wax blends as its applications.
- where: Wire, cable and molding compounds
line: The ExxonMobil EVA 43031.CD datasheet lists crosslinkable compounds, molding compounds, extrusion compounds and wire and cable compounds.
- where: Closed-cell foam
line: Wikipedia says closed-cell EVA foam is used in play mats, sports padding and sports-shoe midsoles.
can_do:
- label: Stiffness
benchmark: flexural_modulus
value: 19 MPa for EVA 150028
line: EVA 150028 has a flexural modulus of 19 MPa (1% secant, ExxonMobil typical value). EVA 43031.CD has 9.6 MPa.
- label: Softness
benchmark: shore_a_hardness
value: 75 Shore A for EVA 150028
line: EVA 150028 has a Shore A hardness of 75 at 15 sec, and EVA 43031.CD has 63.
- label: Stretch
benchmark: elongation
value: 522 % for EVA 150028
line: EVA 150028 elongates 522 % at break. EVA 43031.CD is printed as more than 723 %.
- label: Melting
benchmark: melting_point
value: 66 °C for EVA 150028
line: The datasheet peak melting temperatures are 66 °C for EVA 150028 and 59 °C for EVA 43031.CD. The two SDS ranges are wider, at 35 to 110 °C for the copolymer and 60 to 105 °C for the Hanwha family.
compare: The two ExxonMobil grades differ in vinyl acetate content (27.6 wt% against 31.4 wt%), and that gap shows in their datasheet values. EVA 43031.CD has a higher density (0.955 g/cm3 against 0.945 g/cm3), a lower peak melting temperature (59 °C against 66 °C) and a lower flexural modulus (9.6 MPa against 19 MPa). The SDS melting ranges are wider than either datasheet value, and the sources do not agree on one melting point for EVA, so both values are shown side by side. This profile does not rank EVA against other polymers, because the other profiles use different grades and test conditions.
compare_rows:
- label: Density
benchmark: density
- label: Melt index
benchmark: melt_flow_rate
- label: Vicat softening temperature
benchmark: vicat_softening_temperature
handling:
- Name the grade, because vinyl acetate content changes the melting point, stiffness and density between grades.
- Avoid dust. The ExxonMobil SDS says to vacuum dust with a HEPA filter and not to dry sweep, and it warns of an explosible dust-air mixture.
- Hot material can cause thermal burns, so use protective equipment and cool molten material with cold water.
- Keep away from heat, sparks and flames, and from strong oxidizing agents and amines, per the Hanwha SDS.
- Avoid elevated temperatures for prolonged periods, per the ExxonMobil SDS.
good_for:
- Adhesive and sealant use. EVA 150028 has a melt index of 150 g/10 min at 190 °C/2.16 kg and a peak melting temperature of 66 °C, per its datasheet.
- Flexible parts. EVA 150028 has a Shore A hardness of 75 and an elongation at break of 522 %.
- Wire and cable compounds. EVA 43031.CD is listed for these, with a melt index of 43 g/10 min.
watch_out:
- 'Ageing: the 1983 JPL abstract reports acetic acid among the volatile products at higher temperatures. No retention figure after UV exposure was read.'
- 'Melting range: the datasheets give peak melting temperatures of 66 °C and 59 °C, while the SDS ranges run to 110 °C, so the value depends on the source.'
- 'Carcinogenicity: the ExxonMobil SDS says the product ''May cause cancer'', based on its vinyl acetate component.'
- 'Acetic acid: heat and hydrolysis can form acetic acid, and the SDS lists it among thermal degradation products.'
verdict: 'EVA is a practical, low-melting copolymer whose datasheet values for two ExxonMobil grades are well sourced, but its ageing data are thin: one 1983 abstract, and no flight, erosion or outgassing values for EVA were found in this run.'
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.
| # | Source | Type | Year | Used for |
|---|---|---|---|---|
| Ethylene-vinyl acetate, Wikipedia | web | 3 values | ||
| ExxonMobil EVA 150028, Ethylene Vinyl Acetate Copolymer, product datasheet | datasheet | 2020 | 10 values | |
| ExxonMobil EVA 43031.CD, Ethylene Vinyl Acetate Copolymer, product datasheet | datasheet | 2020 | 10 values | |
| Hanwha Solutions safety data sheet, EVA family, version 2 | datasheet | 2024 | 7 values | |
| ExxonMobil safety data sheet, Ethylene Vinyl Acetate Copolymer, version 8.03 | datasheet | 2026 | 9 values | |
| Photothermal degradation of ethylene/vinylacetate copolymer (Liang et al., Jet Propulsion Laboratory) | paper | 1983 | 3 values | |
| Ethylene, Wikipedia | web | 1 value | ||
| Vinyl acetate, Wikipedia | web | 1 value |
Updated