Titanium carbide TiC

TiC, titanium carbide: a 1:1 titanium-carbon compound with a cubic rock-salt (NaCl-type) structure (Wikipedia, composition only · CAS 12070-08-5 · cubic, Fm-3m

Titanium carbide is a titanium-carbon compound, TiC, with a cubic rock-salt structure (Fm-3m, JMST 2018).

14 sources · Updated 2026-10-26 · CC BY 4.0

Evidence level

2 of 5

Lab-measured

Stiffness

444 GPa

Heat capacity

33.81 J K-1 mol-1

Melting

3290 K

Recipe, share of the weight

  • Ti not statedTitanium
  • C not statedCarbon

Best for

Hard wear coatings and bearing surfaces (NASA records of 1980 and 1988), and cermet cutting tools with a carbide or carbonitride hard phase (Kennametal patent)

Weakest at

Oxidation in air above about 225 °C, and a flammable, dust-explosive powder (NextSDS H228; ICSC 1319). Hardness, thermal conductivity and thermal expansion of monolithic TiC are not sourced in this file

Risk at a glance

  • People None found. Flammable powder, dust-explosion risk (NextSDS, ICSC)
  • If it fails High. Dust cloud ignition
  • Corrosion Moderate. In air, TiC starts to lose intensity above 225 °C and converts to anatase, then rutile TiO2

Quick facts: TiC

Key properties of TiC
PropertyValueBasis
Density4.93 g/cm³1 sourced value
Young's modulus444 GPa1 sourced value
Melting point3,017 to 3,160 °C2 sourced values across conditions

What is the density of Titanium carbide (TiC)?

Titanium carbide (TiC) has a density of 4.93 g/cm³. The source and test conditions are listed in the properties table on this page.

What is the melting point of Titanium carbide (TiC)?

Titanium carbide (TiC) has a melting point of 3,017 to 3,160 °C. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What is the Young's modulus of Titanium carbide (TiC)?

Titanium carbide (TiC) has a Young's modulus of 444 GPa. The source and test conditions are listed in the properties table on this page.

What is Titanium carbide (TiC) used for?

Uses recorded in the sources include Titanium carbide coated steel balls in aerospace ball bearings; Sputtered TiC coating on refractory substrates that form stable nitrides; Cermet cutting tool with a carbonitride hard phase and nickel and cobalt binder (TiC is named in the starting powder list).

Why it exists

Titanium carbide is a hard, high-melting carbide used where wear resistance and heat resistance matter more than toughness. The NASA 1988 record links TiC-coated steel balls to better bearing life in oil-lubricated and oil-free bearings, and the 1980 NASA record describes TiC sputtered coatings that bond well to refractory substrates. The JANAF table gives a standard enthalpy of formation of -184.096 kJ/mol for the crystalline solid, and a WebQC density of 4.9300 g/cm3.

Where it's used

Bearing surfaces

A 1988 NASA record says TiC-coated steel balls can bring large gains in performance and life in both oil-grease lubricated and oil-grease free bearings. The abstract gives no test numbers.

Wear and adhesion coatings

A 1980 NASA Lewis record describes sputtering TiC onto refractory substrates, with a short nitrogen step to bond the coating. The record describes better adhesion, friction and wear.

Cermet cutting tools

A 1990 Kennametal patent describes cermet cutting tools for turning AISI 1045 and 4340 steels. The claimed hard phase is titanium carbonitride, so this is a relative of TiC rather than pure TiC.

Recipe

TiC, titanium carbide: a 1:1 titanium-carbon compound with a cubic rock-salt (NaCl-type) structure (Wikipedia, composition only; JMST 2018 gives Fm-3m)

TiC is a titanium-carbon compound with one titanium and one carbon per formula unit (JANAF; Wikipedia for the composition name). It has a cubic rock-salt structure, Fm-3m (JMST 2018). Synthesis route not sourced in this file.

What TiC is made of
IngredientShare of the weightWhat it does
Titanium Ti not stated Metal sublattice of the rock-salt structure (JMST 2018 gives Fm-3m for TiC).
Carbon C not stated Interstitial sublattice of the rock-salt structure, with the titanium-carbon bonding that gives the carbide its hardness and heat resistance.

Weight shares are as printed in the sources.

What it can do

Stiffness

444 GPa

worked out from the formula

The first-principles elastic modulus is 444 GPa at zero pressure (JMST 2018). It is calculated, not measured, and is the only stiffness value in this file.

Heat capacity

33.81 J K-1 mol-1

measured

The crystalline solid has a molar heat capacity of 33.807 J K-1 mol-1 at 298.15 K and 51.179 J K-1 mol-1 at 1000 K (JANAF).

Melting

3290 K

measured

JANAF gives a crystal-to-liquid transition at 3290 K. WebQC gives a melting point of 3160.00 °C. The two sources disagree, so both are shown.

How it compares

The JANAF transition (3290 K) and the WebQC melting point (3160.00 °C) are different values, and both are kept. The calculated elastic modulus (444 GPa), bulk modulus (268 GPa) and shear modulus (181 GPa) are first-principles values for an ideal crystal. They do not replace measured stiffness data. The compare rows are the three values available from sources read in this run.

The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.

Benchmarks
MeasurementTiCAl4C3B4CHfCMAXMo2CNbCSiCTaCZrC
Capacity and energy
Molar heat capacity Cp, TiC, 298.15 K33.81 J K-1 mol-11116.8 J K-1 mol-153.76 J K-1 mol-1no datano datano data36.23 J K-1 mol-1no datano datano data
Molar heat capacity Cp, TiC, 1000 K51.18 J K-1 mol-12116.8 J K-1 mol-153.76 J K-1 mol-1no datano datano data36.23 J K-1 mol-1no datano datano data
Standard Gibbs energy of formation, TiC, 298.15 KJANAF table value at 298.15 K; delta-f G column-180.4 kJ mol-15-203.4 kJ mol-1no datano datano datano data-136.8 kJ mol-1no datano datano data
Thermal behavior and safety
Crystal-to-liquid transition, TiC (JANAF)3290 K62100 °Cno data3890 °C1663 K2687 °C3608 °Cno data3880 °C3532 °C
Melting point, TiC (WebQC)3160 °C72100 °Cno data3890 °C1663 K2687 °C3608 °Cno data3880 °C3532 °C
Physical and electrical
Density, TiC (WebQC)4.93 g/cm³82.36 g/cm³2.5 gm/cm³12.2 g/cm³4.47 g/cm³9.18 g/cm³7.82 g/cm³3.08 g/cm³14.5 g/cm³6.73 g/cm³
Other measurements
Standard molar entropy S, TiC, 298.15 K24.23 J K-1 mol-1388.97 J K-1 mol-127.18 J K-1 mol-1no datano datano data34.97 J K-1 mol-1no datano datano data
Standard enthalpy of formation, TiC, 298.15 KJANAF table value at 298.15 K; delta-f H column-184.1 kJ mol-14-215.7 kJ mol-1-62.68 kJ mol-1no datano datano data-138.9 kJ mol-1no datano datano data
Molar mass, TiC (WebQC)59.88 g/mol9144 g/molno datano datano datano data104.9 g/molno datano datano data
Elastic modulus, TiC, first-principles, zero pressure444 GPa10no data440 GPano data265 GPano datano data395 GPano data435 GPa
Bulk modulus, TiC, first-principles, zero pressure268 GPa11no datano datano data135 GPano datano datano datano datano data
Shear modulus, TiC, first-principles, zero pressure181 GPa12no datano datano data113 GPano datano datano datano datano data

Why choose it, and why not

Good for

  • Wear and bearing surfaces. The 1988 NASA record reports large gains in bearing life with TiC-coated steel balls.
  • High-melting carbide. JANAF places the crystal-to-liquid transition at 3290 K.

Watch out for

  • Oxidation in air above about 225 °C, with rutile TiO2 forming and the carbide lost.
  • A flammable powder that can form explosive dust clouds (NextSDS H228; ICSC 1319).
  • Melting point and hardness are not settled here. The melting values differ by source, and hardness, thermal conductivity and thermal expansion were not sourced.

Titanium carbide is a high-melting, stiff carbide with JANAF thermochemistry and calculated elastic constants. Its bearing and coating uses have NASA support, and its air oxidation onset is measured. Its powder hazard is a dust-explosion risk. Hardness, thermal conductivity and thermal expansion of monolithic TiC are not yet sourced.

Technical details

For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.

Notes

The method, full conditions and any caveat for the numbered rows above.

Notes for the numbered rows
#MeasurementMethodConditionsCaveat
1Molar heat capacity Cp, TiC, 298.15 KJANAF table value at 298.15 K; molar, so not converted to the canonical specific heat (no molar mass conversion applied in this file)temperature 298.15 Kreference state standard state pressure 0.1 MPaphase crystalline (cr)—
2Molar heat capacity Cp, TiC, 1000 KJANAF table value at 1000 K, read from the same tabletemperature 1000 Kreference state standard state pressure 0.1 MPaphase crystalline (cr)—
3Standard molar entropy S, TiC, 298.15 KJANAF table value at 298.15 K; column mapped from the table layouttemperature 298.15 Kreference state standard state pressure 0.1 MPaphase crystalline (cr)—
4Standard enthalpy of formation, TiC, 298.15 K—temperature 298.15 Kreference state standard state pressure 0.1 MPaphase crystalline (cr)—
5Standard Gibbs energy of formation, TiC, 298.15 K—temperature 298.15 Kreference state standard state pressure 0.1 MPaphase crystalline (cr)—
6Crystal-to-liquid transition, TiC (JANAF)JANAF lists the crystal-liquid transition as a temperature row in the table; it is not labelled as a melting point. The value is kept in kelvin as printedbasis JANAF crystal-liquid transition rowreference state standard state pressure 0.1 MPa—
7Melting point, TiC (WebQC)WebQC physical-properties value; the site does not name its original sourcebasis as printed by WebQC—
8Density, TiC (WebQC)WebQC physical-properties value; printed as 4.9300 g/cm³ and written here as g/cm3basis as printed by WebQC (4.9300 g/cm3)—
9Molar mass, TiC (WebQC)WebQC property block, Properties of Titanium carbide headingbasis molar mass of TiC as printed by WebQC—
10Elastic modulus, TiC, first-principles, zero pressureFirst-principles calculation as printed in JMST 2018 Table 3. Calculated, not measuredpressure 0 GPastructure Fm-3m—
11Bulk modulus, TiC, first-principles, zero pressureFirst-principles calculation as printed in JMST 2018 Table 3. Calculated, not measuredpressure 0 GPastructure Fm-3m—
12Shear modulus, TiC, first-principles, zero pressureFirst-principles calculation as printed in JMST 2018 Table 3. Calculated, not measuredpressure 0 GPastructure Fm-3m—

Corrosion and compatibility

What happens when it meets other materials and environments.

Corrosion and compatibility
EnvironmentConcernWhat happens
Air, in-situ XRD on the smaller TiC particles, room temperature to 1000 °C moderate In air, TiC starts to lose intensity above 225 °C and converts to anatase, then rutile TiO21
Oxygen, thermogravimetry with DSC steps at 5, 10 and 20 K/min up to 1500 °C moderate In oxygen, TiC oxidation runs in steps, the first at about 482 to 492 °C2
Air, isothermal exposure at 600 to 1150 °C for up to 1140 hours not rated Isothermal oxidation converts TiC fully to rutile, with a first-order kinetic fit3
Corrosion details
#EnvironmentDetailsTest conditions
1 Air, in-situ XRD on the smaller TiC particles, room temperature to 1000 °C The TiC XRD intensity decreases above 225 °C. Anatase forms above 350 °C, rutile is detected at 580 °C, and rutile exceeds anatase at 800 °C. No brookite or other intermediate was detected. The initial rise up to 225 °C is attributed to preferred orientation. The rating moderate is the assistant's judgement from these onset temperatures; the paper gives no rating. atmosphere airsample TiC4, the smaller particle sizetemperature room temperature to 1000 °C, 25 K steps
2 Oxygen, thermogravimetry with DSC steps at 5, 10 and 20 K/min up to 1500 °C At 5 K/min the DSC reaction steps are at 482, 708 and 837 °C for TiC4, and at 492, 740, 916 and 1036 °C for TiC150. For the small particles the mass increase shifts to higher temperature as the heating rate rises. The theoretical maximum mass increase on complete oxidation is 33.4 mass percent. The rating moderate is the assistant's judgement; the paper gives no rating. atmosphere oxygenheating rates 5, 10 and 20 K/mintemperature up to 1500 °C
3 Air, isothermal exposure at 600 to 1150 °C for up to 1140 hours XRD shows oxidation of TiC to rutile in every isothermal sample, with no by-products or intermediates detected. A first-order fit gives an activation energy of 117.3 kJ/mol and log A of 4.3 (1/s). Each is printed with a decimal comma in the source. The paper gives no rate in mass or thickness units, so the rating is unknown. atmosphere airtemperature 600 to 1150 °Ctime up to 1140 hours

Risks and side effects

Hazards to people, what happens when a cell overheats, and how the material is handled and stored.

For people

The powder is flammable as a solid, and a dispersed dust cloud can explode. Treat dust as the main hazard until a manufacturer's safety data sheet is read.

Dust
ICSC 1319 says finely dispersed particles form explosive mixtures in air, and that repeated or prolonged inhalation of dust may affect the lungs. Prevent dispersion of dust.
Flammability
NextSDS gives H228, flammable solid, with GHS02. Keep the powder away from sparks, and use explosion-proof electrical and ventilating equipment (P241).

If a part or powder heats up

These numbers come from the Fraunhofer oxidation study of TiC particles in air and oxygen.

In air
TiC intensity starts to fall above 225 °C. Anatase forms above 350 °C and rutile at 580 °C.
In oxygen
At 5 K/min the first reaction step is at 482 °C for the smaller particles and 492 °C for the larger ones.

Test details
The original wording and numbers from the sources, for readers who want them.

Failure risks

Failure risks
FailureTrigger and consequence
Dust cloud ignitionhigh severityPowder dispersed in air near an ignition source or sparkICSC 1319 says finely dispersed particles form explosive mixtures in air. The card prints no exposure limit.
Conversion of the carbide to TiO2 at high temperaturemoderate severityHeating in air above about 225 °C, or in oxygen above about 482 °C at 5 K/minLoss of the TiC phase and formation of rutile TiO2; the full oxidation adds up to 33.4 mass percent to the sample

Handling and storage

  • ICSC 1319: prevent dispersion of dust. A harmful concentration of airborne particles can be reached quickly when the powder is dispersed, and repeated or prolonged inhalation of dust may affect the lungs.
  • NextSDS Section 02 precautionary statement P241: use explosion-proof electrical, ventilating and lighting equipment.

Supply and geography

How common the raw materials are and where they come from.

Titanium (feedstock for the titanium half of TiC)

5650 ppm in the Earth's crust (USGS PP 1802-A Table A1, citing Jefferson Science Associates 2014). USGS 2026: no U.S. sponge production in 2025; imports were an estimated 44000 t in 2025e.

Top producers (2025)
China 70.3%, Japan 14.3%, Russia 6.8%, Kazakhstan 4.3%, Saudi Arabia 3.2%
Critical mineral lists
US: listed, EU: listed
Recycling
USGS 2026: consumption data for titanium scrap metal for the titanium metal industry were withheld, because survey responses were limited.
Substitutes
USGS 2026: few materials match titanium metal's strength-to-weight ratio and corrosion resistance. Aluminum, nickel, specialty steels and zirconium alloys may replace titanium where corrosion resistance is needed. This is about titanium metal, not TiC.