Molybdenum carbide Mo2C
Mo2C, molybdenum carbide: a 2:1 molybdenum-carbon compound. MoC is the other composition that Wikipedia lists for the same system · CAS 12069-89-5
Molybdenum carbide is a molybdenum-carbon compound.
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Melting
2687 °C
Density
9.18 g/cm³
Hydrogen evolution
83 mV dec-1
Recipe, share of the weight
- Mo 94.1%Molybdenum
- C 5.9%Carbon
Best for
Hard, high-melting carbide powder for wear parts and tool materials (vendor claims), and noble-metal-free hydrogen-evolution electrocatalysis in both acid and alkaline water (Hussain et al. 2019)
Weakest at
Hardness, thermal conductivity and expansion of pure Mo2C are not sourced in this file. The powder oxidises in steam or CO2 from about 600 °C, and it is a dust-forming powder that the SDS says to keep from dispersing
Risk at a glance
- People None found. Not classed hazardous, but dust must be kept down
- If it fails Moderate. Oxidation of the carbide at high temperature
- Corrosion Moderate. In steam or CO2, Mo2C oxidation starts at about 600 °C
Quick facts: Mo2C
| Property | Value | Basis |
|---|---|---|
| Density | 9.18 to 9.2 g/cm³ | 2 sourced values across conditions |
| Melting point | 2,687 to 2,690 °C | 2 sourced values across conditions |
What is the density of Molybdenum carbide (Mo2C)?
Molybdenum carbide (Mo2C) has a density of 9.18 to 9.2 g/cm³. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the melting point of Molybdenum carbide (Mo2C)?
Molybdenum carbide (Mo2C) has a melting point of 2,687 to 2,690 °C. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is Molybdenum carbide (Mo2C) used for?
Uses recorded in the sources include Superhard tool material and wear-resistant parts; Electrocatalyst for hydrogen evolution in water electrolysis.
Why it exists
Molybdenum carbide is a dense, high-melting carbide with two sourced uses. A vendor describes the powder as a superhard tool material and a wear-resistant material, with no test data. Hussain et al. (2019) show that chemically reduced Mo2C nanoparticles on nickel foam are an active, noble-metal-free electrocatalyst for hydrogen evolution in both acid and alkaline water. Its composition and phase names come from Wikipedia, which is used for composition and history only.
Where it's used
Wear and tool materials
A vendor page lists Mo2C powder as a superhard tool material and a wear-resistant material. The page gives no test numbers.
Hydrogen-evolution electrocatalyst
In 0.5 M H2SO4 the Mo2C catalyst reaches 10 mA cm-2 at -134 mV, with a Tafel slope of 83 mV dec-1. In 1 M KOH it reaches the same current density at -116 mV, with a Tafel slope of 65 mV dec-1 (Hussain et al. 2019).
Catalysis in general
A vendor page says Mo2C is used as a catalyst for reactions involving hydrogen, such as alkane isomerisation. No primary source for this use was read in this run.
Recipe
Mo2C, molybdenum carbide: a 2:1 molybdenum-carbon compound. MoC is the other composition that Wikipedia lists for the same system
Mo2C is a molybdenum-carbon compound with two molybdenum atoms and one carbon atom per formula unit. Wikipedia lists MoC and Mo2C as the two compositions of this system, with at least three phases. The synthesis route is not sourced in this file.
| Ingredient | Atoms per unit | Share of the weight | What it does |
|---|---|---|---|
| Molybdenum Mo | 2 | 94.1% | The metal sublattice. The NIST standard atomic weight is 95.95 with an uncertainty of 1 in the last digit. |
| Carbon C | 1 | 5.9% | Sits in the interstitial sites of the metal lattice. NIST prints the standard atomic weight as the interval 12.0096 to 12.0116, and the lower bound is used. |
Weight shares are calculated from standard atomic weights.
What it can do
Melting
2687 °C
measured
The SDS gives a melting point of 2687 °C. The Nanografi micron powder is listed at 2690 °C. The two are kept side by side.
Density
9.18 g/cm³
measured
Two vendors list 9.18 g/cm3 and 9.20 g/cm3. No measurement method is given by either vendor.
Hydrogen evolution
83 mV dec-1
measured
At 10 mA cm-2 the overpotential is -134 mV in 0.5 M H2SO4 and -116 mV in 1 M KOH, with the catalyst on nickel foam (Hussain et al. 2019). These depend on electrolyte and substrate.
How it compares
The Mo2C densities from two vendors (9.18 and 9.20 g/cm3) are higher than the density of titanium carbide in its own profile, and the Mo2C melting point (2687 °C in the SDS) is also high for a carbide. The HER overpotential is only meaningful against other catalysts in the same electrolyte and on the same substrate, so no cross-catalyst ranking is made here. Molybdenum diboride (MoB2) is a related molybdenum boride, mentioned here for context only and not profiled in this file.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | Mo2C | Al4C3 | B4C | HfC | MAX | NbC | SiC | TaC | TiC | ZrC |
|---|---|---|---|---|---|---|---|---|---|---|
| Thermal behavior and safety | ||||||||||
| Melting point, Mo2C (SDS) | 2687 °C3 | 2100 °C | no data | 3890 °C | 1663 K | 3608 °C | no data | 3880 °C | 3290 K | 3532 °C |
| Melting point, Mo2C micron powder (Nanografi) | 2690 °C4 | 2100 °C | no data | 3890 °C | 1663 K | 3608 °C | no data | 3880 °C | 3290 K | 3532 °C |
| Physical and electrical | ||||||||||
| Density, Mo2C powder (SAMaterials product page) | 9.18 g/cm³1 | 2.36 g/cm³ | 2.5 gm/cm³ | 12.2 g/cm³ | 4.47 g/cm³ | 7.82 g/cm³ | 3.08 g/cm³ | 14.5 g/cm³ | 4.93 g/cm³ | 6.73 g/cm³ |
| Density, Mo2C micron powder (Nanografi) | 9.2 g/cm³2 | 2.36 g/cm³ | 2.5 gm/cm³ | 12.2 g/cm³ | 4.47 g/cm³ | 7.82 g/cm³ | 3.08 g/cm³ | 14.5 g/cm³ | 4.93 g/cm³ | 6.73 g/cm³ |
| Exchange current density, Mo2C in 0.5 M H2SO4 | 0.131 mA cm-27 | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Exchange current density, Mo2C in 1 M KOH | 0.846 mA cm-28 | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Other measurements | ||||||||||
| Tafel slope, Mo2C in 0.5 M H2SO4 | 83 mV dec-15 | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Tafel slope, Mo2C in 1 M KOH | 65 mV dec-16 | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Turnover frequency, Mo2C at -134 mV in acid | 0.005 H2 s-19 | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Turnover frequency, Mo2C at -116 mV in alkaline | 0.037 H2 s-110 | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Particle size D50, Mo2C powder (SAMaterials product page) | 0.5 µm11 | no data | no data | no data | no data | no data | no data | no data | no data | no data |
Why choose it, and why not
Good for
- Hard, high-melting powder for wear parts and tool materials, as claimed by the vendor. No test data are sourced here.
- Noble-metal-free electrocatalysis for hydrogen evolution in acid and alkaline water, per Hussain et al. 2019.
Watch out for
- Oxidation in steam or CO2 from about 600 °C, and oxycarbide formation under oxygen-bearing conditions (Likith et al. 2018).
- The SDS does not fully investigate toxicology, and the dust must be kept down even though the powder is not classed as hazardous.
- China imposed export controls on molybdenum powders in February 2025 (USGS MCS 2026). This affects supply of the feedstock, not the Mo2C itself.
- Hardness, thermal conductivity and expansion of pure Mo2C are not settled here.
Molybdenum carbide is a high-melting, dense carbide with a sourced hydrogen-evolution record and a vendor-stated use as a tool and wear material. Its hardness, thermal properties and air oxidation kinetics are not sourced in this file. The powder is classed as not hazardous, but its toxicology is not fully investigated and it oxidises from about 600 °C in steam or CO2.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Density, Mo2C powder (SAMaterials product page) | Vendor specification value, read from the product specification table. The vendor does not name a measurement method. | form powder, purity more than 99.5 percent as printedbasis vendor specification table | — |
| 2 | Density, Mo2C micron powder (Nanografi) | Vendor specification value. It differs from the 9.18 g/cm3 printed by the other vendor, and no method is given by either. | form micron powder, average particle size 2.6 µm as printedbasis vendor specification list | — |
| 3 | Melting point, Mo2C (SDS) | Supplier SDS value, printed as 2687 °C. The Fahrenheit equivalent on the same row is not used. | basis as printed in SDS section 9 | — |
| 4 | Melting point, Mo2C micron powder (Nanografi) | Vendor specification value, printed as 2690.0 °C. It is 3 °C above the SDS value of 2687 °C, and the two are kept side by side. | basis as printed on the vendor specification list | — |
| 5 | Tafel slope, Mo2C in 0.5 M H2SO4 | Tafel plot from the linear sweep data. The authors read the Volmer-Heyrovsky step from this slope. | electrolyte 0.5 M H2SO4form chemically reduced Mo2C nanoparticles on nickel foam | — |
| 6 | Tafel slope, Mo2C in 1 M KOH | Tafel plot from the linear sweep data, as tabulated by the authors. | electrolyte 1 M KOHform chemically reduced Mo2C nanoparticles on nickel foam | — |
| 7 | Exchange current density, Mo2C in 0.5 M H2SO4 | Value tabulated by the authors, read from the exchange current density column. | electrolyte 0.5 M H2SO4form chemically reduced Mo2C nanoparticles on nickel foam | — |
| 8 | Exchange current density, Mo2C in 1 M KOH | Value tabulated by the authors, read from the exchange current density column. | electrolyte 1 M KOHform chemically reduced Mo2C nanoparticles on nickel foam | — |
| 9 | Turnover frequency, Mo2C at -134 mV in acid | Calculated by the authors from the number of active sites. It is a per-site rate, not a mass rate. | electrolyte 0.5 M H2SO4overpotential -134 mV | — |
| 10 | Turnover frequency, Mo2C at -116 mV in alkaline | Calculated by the authors from the number of active sites. It is a per-site rate, not a mass rate. | electrolyte 1 M KOHoverpotential -116 mV | — |
| 11 | Particle size D50, Mo2C powder (SAMaterials product page) | Vendor specification range, printed as 0.5-3 µm. This is the vendor micron powder, not the Nanografi sample. | basis APS (D50) as printed by the vendor | — |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Steam or carbon dioxide at high temperature, up to 850 °C and up to 8 bar | moderate | In steam or CO2, Mo2C oxidation starts at about 600 °C1 |
| Air or storage at room temperature | not rated | The SDS calls Mo2C stable under normal conditions; no air oxidation rate was read2 |
| Oxygen-bearing surfaces during deoxygenation (DFT on the Mo2C(100) surface) | not rated | Oxygen deposited on Mo2C can form oxycarbides3 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Steam or carbon dioxide at high temperature, up to 850 °C and up to 8 bar | Darujati (2002) reports an oxidation onset of about 600 °C in either steam or CO2. Above 750 °C the paper describes thermal decomposition and then oxidation of the Mo metal. CO2 is the stronger oxidant at the higher temperatures. The rating moderate is the assistant's judgement from this onset; the paper gives no rating. | atmosphere steam or CO2pressure up to 8 bartemperature up to 850 °C |
| 2 | Air or storage at room temperature | The SDS section 10 says the product is stable under normal conditions, with no known reactive hazard, and lists oxidising agents as incompatible. No onset temperature or mass gain for Mo2C powder in air was found in a source read in this run, so the rating is unknown. | atmosphere airtemperature normal storage |
| 3 | Oxygen-bearing surfaces during deoxygenation (DFT on the Mo2C(100) surface) | Likith et al. (2018) state that oxygen deposited during deoxygenation reactions may alter the carbide structure and form oxycarbides. Their surface calculations suggest that oxygen is not stable under the top Mo layer of the Mo2C(100) surface. The rating is unknown because the paper gives no corrosion rate. | basis DFT surface calculations on Mo2C(100) |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
The supplier SDS classes the powder as not hazardous under OSHA 2012, but the toxicology has not been fully investigated. Treat the dust as the main handling concern.
- Dust
- The SDS says to avoid dust formation. It lists an ACGIH TLV of 10 mg/m3 as a TWA.
- Toxicology
- The SDS states that the toxicological properties have not been fully investigated, and gives no irritation or sensitization data.
If the powder heats in steam or CO2
These numbers come from the Darujati thesis on Mo2C oxidation in steam and CO2.
- Onset
- Oxidation starts at about 600 °C in either steam or CO2. Above 750 °C the paper describes decomposition and then oxidation of the Mo metal.
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Oxidation of the carbide at high temperaturemoderate severity | Heating in steam or CO2 above about 600 °CConversion of the carbide to oxide. Above 750 °C the paper describes decomposition followed by oxidation of the Mo metal. |
| Reaction with oxidising agentslow severity | Contact with an oxidising agentThe SDS lists oxidising agents as incompatible. Hazardous decomposition products are molybdenum oxides. |
| Oxycarbide formation on the surfacelow severity | Oxygen deposited during deoxygenation reactionsMay alter the carbide structure and form oxycarbides, per Likith et al. (2018). The effect on performance is not quantified in the abstract. |
Handling and storage
- Keep the powder from dispersing. The SDS says to avoid dust formation during handling and clean-up, and to ventilate the area.
- Store in a dry, cool and well-ventilated place with the containers tightly closed, away from oxidising agents (SDS section 7).
- Wear eye protection and gloves. The SDS lists a particle filter for respiratory protection and says no protective equipment is needed under normal use conditions.
Supply and geography
How common the raw materials are and where they come from.
Molybdenum (feedstock for the molybdenum half of Mo2C)
Not in the USGS PP 1802-A Table A1 crustal abundance list, which has no molybdenum row. The same table lists carbon at 200 ppm.
- Top producers (2025)
- China 37.3%, Chile 16.2%, United States 15.4%, Peru 15%, Mexico 6.5%
- Recycling
- USGS 2026: molybdenum is recycled as a component of catalysts, ferrous scrap and superalloy scrap.
- Substitutes
- USGS 2026: little substitution for molybdenum in steels and cast irons. Potential substitutes in alloy steels include boron, chromium, niobium and vanadium, and tungsten in tool steels.
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: molybdenum-carbide
spore_version: 0.2
family: carbide-nitride-boride-ceramics
name: Molybdenum carbide
abbreviation: Mo2C
role: hard refractory carbide for wear parts and tool materials, and a noble-metal-free electrocatalyst for hydrogen evolution
category: ceramics
type: carbides
summary: |
Molybdenum carbide is a molybdenum-carbon compound. Wikipedia lists two formulas, Mo2C and MoC, and at least three phases, including beta-Mo2C and gamma-MoC. A supplier SDS (revision 30-Mar-2024) gives a melting point of 2687 °C for Mo2C, and two vendors give a density of 9.18 g/cm3 and 9.20 g/cm3. In Hussain et al. (2019), chemically reduced Mo2C nanoparticles on nickel foam reach 10 mA cm-2 at -134 mV in 0.5 M H2SO4 and at -116 mV in 1 M KOH, for hydrogen evolution. A 2002 Washington State University thesis reports an oxidation onset near 600 °C in steam or CO2. The supplier SDS classes the powder as not hazardous under the 2012 OSHA standard, but says its toxicological properties have not been fully investigated. Molybdenum diboride (MoB2) is a related molybdenum boride, mentioned here only for context and not profiled in this file.
best_for: Hard, high-melting carbide powder for wear parts and tool materials (vendor claims), and noble-metal-free hydrogen-evolution electrocatalysis in both acid and alkaline water (Hussain et al. 2019)
weakest_at: Hardness, thermal conductivity and expansion of pure Mo2C are not sourced in this file. The powder oxidises in steam or CO2 from about 600 °C, and it is a dust-forming powder that the SDS says to keep from dispersing
identity:
formula: 'Mo2C, molybdenum carbide: a 2:1 molybdenum-carbon compound. MoC is the other composition that Wikipedia lists for the same system'
cas: 12069-89-5
source: sam-mo2c-sds
where: Section 3 Composition, Molybdenum carbide (Mo2C), CAS No 12069-89-5
tags:
environments: []
stresses:
- extreme-heat
applications:
- mechanisms
- cryogenic-fuel
properties:
- benchmark: density
label: Density, Mo2C powder (SAMaterials product page)
value: 9.18
unit: g/cm3
scope: material
conditions:
form: powder, purity more than 99.5 percent as printed
basis: vendor specification table
method: Vendor specification value, read from the product specification table. The vendor does not name a measurement method.
status: ground
source: sam-mo2c-product
where: Product specification table, Density (g/cm3) row
- benchmark: density
label: Density, Mo2C micron powder (Nanografi)
value: 9.2
unit: g/cm3
scope: material
conditions:
form: micron powder, average particle size 2.6 µm as printed
basis: vendor specification list
method: Vendor specification value. It differs from the 9.18 g/cm3 printed by the other vendor, and no method is given by either.
status: ground
source: nanografi-mo2c
where: Product specification list, density row
- benchmark: melting_point
label: Melting point, Mo2C (SDS)
value: 2687
unit: °C
scope: material
conditions:
basis: as printed in SDS section 9
method: Supplier SDS value, printed as 2687 °C. The Fahrenheit equivalent on the same row is not used.
status: ground
source: sam-mo2c-sds
where: Section 9 Physical and chemical properties, Melting Point/Range row
- benchmark: melting_point
label: Melting point, Mo2C micron powder (Nanografi)
value: 2690
unit: °C
scope: material
conditions:
basis: as printed on the vendor specification list
method: Vendor specification value, printed as 2690.0 °C. It is 3 °C above the SDS value of 2687 °C, and the two are kept side by side.
status: ground
source: nanografi-mo2c
where: Product specification list, melting point row
- benchmark: tafel_slope
label: Tafel slope, Mo2C in 0.5 M H2SO4
value: 83
unit: mV dec-1
scope: material
conditions:
electrolyte: 0.5 M H2SO4
form: chemically reduced Mo2C nanoparticles on nickel foam
method: Tafel plot from the linear sweep data. The authors read the Volmer-Heyrovsky step from this slope.
status: ground
source: hussain-2019
where: Table 1, row 0.5 M H2SO4, Mo2C, Tafel slope column; text on the Tafel slope
- benchmark: tafel_slope
label: Tafel slope, Mo2C in 1 M KOH
value: 65
unit: mV dec-1
scope: material
conditions:
electrolyte: 1 M KOH
form: chemically reduced Mo2C nanoparticles on nickel foam
method: Tafel plot from the linear sweep data, as tabulated by the authors.
status: ground
source: hussain-2019
where: Table 1, row 1 M KOH, Mo2C, Tafel slope column
- benchmark: exchange_current_density
label: Exchange current density, Mo2C in 0.5 M H2SO4
value: 0.131
unit: mA cm-2
scope: material
conditions:
electrolyte: 0.5 M H2SO4
form: chemically reduced Mo2C nanoparticles on nickel foam
method: Value tabulated by the authors, read from the exchange current density column.
status: ground
source: hussain-2019
where: Table 1, row 0.5 M H2SO4, Mo2C, exchange current density column
- benchmark: exchange_current_density
label: Exchange current density, Mo2C in 1 M KOH
value: 0.846
unit: mA cm-2
scope: material
conditions:
electrolyte: 1 M KOH
form: chemically reduced Mo2C nanoparticles on nickel foam
method: Value tabulated by the authors, read from the exchange current density column.
status: ground
source: hussain-2019
where: Table 1, row 1 M KOH, Mo2C, exchange current density column
- benchmark: turnover_frequency
label: Turnover frequency, Mo2C at -134 mV in acid
value: 0.005
unit: H2 s-1
scope: material
conditions:
electrolyte: 0.5 M H2SO4
overpotential: '-134 mV'
method: Calculated by the authors from the number of active sites. It is a per-site rate, not a mass rate.
status: ground
source: hussain-2019
where: Text paragraph after Table 1, TOF values of Mo2C
- benchmark: turnover_frequency
label: Turnover frequency, Mo2C at -116 mV in alkaline
value: 0.037
unit: H2 s-1
scope: material
conditions:
electrolyte: 1 M KOH
overpotential: '-116 mV'
method: Calculated by the authors from the number of active sites. It is a per-site rate, not a mass rate.
status: ground
source: hussain-2019
where: Text paragraph after Table 1, TOF values of Mo2C
- benchmark: particle_size
label: Particle size D50, Mo2C powder (SAMaterials product page)
value: 0.5
value_high: 3
unit: µm
scope: material
conditions:
basis: APS (D50) as printed by the vendor
method: Vendor specification range, printed as 0.5-3 µm. This is the vendor micron powder, not the Nanografi sample.
status: ground
source: sam-mo2c-product
where: Product specification table, APS (D50) row
corrosion:
- environment: Steam or carbon dioxide at high temperature, up to 850 °C and up to 8 bar
headline: In steam or CO2, Mo2C oxidation starts at about 600 °C
effect: Darujati (2002) reports an oxidation onset of about 600 °C in either steam or CO2. Above 750 °C the paper describes thermal decomposition and then oxidation of the Mo metal. CO2 is the stronger oxidant at the higher temperatures. The rating moderate is the assistant's judgement from this onset; the paper gives no rating.
rating: moderate
conditions:
atmosphere: steam or CO2
pressure: up to 8 bar
temperature: up to 850 °C
source: darujati-2002
where: Abstract
- environment: Air or storage at room temperature
headline: The SDS calls Mo2C stable under normal conditions; no air oxidation rate was read
effect: The SDS section 10 says the product is stable under normal conditions, with no known reactive hazard, and lists oxidising agents as incompatible. No onset temperature or mass gain for Mo2C powder in air was found in a source read in this run, so the rating is unknown.
rating: unknown
conditions:
atmosphere: air
temperature: normal storage
source: sam-mo2c-sds
where: Section 10 Stability and reactivity
- environment: Oxygen-bearing surfaces during deoxygenation (DFT on the Mo2C(100) surface)
headline: Oxygen deposited on Mo2C can form oxycarbides
effect: Likith et al. (2018) state that oxygen deposited during deoxygenation reactions may alter the carbide structure and form oxycarbides. Their surface calculations suggest that oxygen is not stable under the top Mo layer of the Mo2C(100) surface. The rating is unknown because the paper gives no corrosion rate.
rating: unknown
conditions:
basis: DFT surface calculations on Mo2C(100)
source: likith-2018
where: Abstract
risks:
hazards:
- text: 'Stanford Advanced Materials SDS, revision 30-Mar-2024: not considered hazardous under the 2012 OSHA Hazard Communication Standard. Label elements none required. Hazards not otherwise classified none identified.'
ghs: []
source: sam-mo2c-sds
where: Section 2 Hazard(s) identification
- text: 'The SDS states that the toxicological properties have not been fully investigated. Irritation and sensitization: no information available.'
source: sam-mo2c-sds
where: Section 11 Toxicological information
- text: 'Exposure guideline printed for Mo2C: ACGIH TLV TWA 10 mg/m3, a second TWA of 3 mg/m3 on the same row, and NIOSH IDLH 5000 mg/m3. The table does not label the second TWA.'
source: sam-mo2c-sds
where: Section 8 Exposure guidelines table
failure_risks:
- mode: Oxidation of the carbide at high temperature
trigger: Heating in steam or CO2 above about 600 °C
consequence: Conversion of the carbide to oxide. Above 750 °C the paper describes decomposition followed by oxidation of the Mo metal.
severity: moderate
source: darujati-2002
where: Abstract
- mode: Reaction with oxidising agents
trigger: Contact with an oxidising agent
consequence: The SDS lists oxidising agents as incompatible. Hazardous decomposition products are molybdenum oxides.
severity: low
source: sam-mo2c-sds
where: Section 7 Storage and Section 10 Stability and reactivity
- mode: Oxycarbide formation on the surface
trigger: Oxygen deposited during deoxygenation reactions
consequence: May alter the carbide structure and form oxycarbides, per Likith et al. (2018). The effect on performance is not quantified in the abstract.
severity: low
source: likith-2018
where: Abstract
side_effects: []
handling:
- text: Keep the powder from dispersing. The SDS says to avoid dust formation during handling and clean-up, and to ventilate the area.
source: sam-mo2c-sds
where: Sections 6 and 7 Accidental release and Handling
- text: Store in a dry, cool and well-ventilated place with the containers tightly closed, away from oxidising agents (SDS section 7).
source: sam-mo2c-sds
where: Section 7 Storage
- text: Wear eye protection and gloves. The SDS lists a particle filter for respiratory protection and says no protective equipment is needed under normal use conditions.
source: sam-mo2c-sds
where: Section 8 Personal protection
mitigations: []
uses:
- application: mechanisms
device: Superhard tool material and wear-resistant parts
example: The vendor product page lists Mo2C powder as a superhard tool material and a wear-resistant material. The page gives no test numbers, so this is a vendor claim only.
source: sam-mo2c-product
where: Applications section
- application: cryogenic-fuel
device: Electrocatalyst for hydrogen evolution in water electrolysis
example: Chemically reduced Mo2C nanoparticles on nickel foam reach 10 mA cm-2 at -134 mV in 0.5 M H2SO4 and at -116 mV in 1 M KOH. This is Earth-side water electrolysis. The application tag cryogenic-fuel is the closest item in the allowed list, not a flight use.
source: hussain-2019
where: Table 1 and abstract
supply:
- subject: Molybdenum (feedstock for the molybdenum half of Mo2C)
abundance: Not in the USGS PP 1802-A Table A1 crustal abundance list, which has no molybdenum row. The same table lists carbon at 200 ppm.
producers:
- country: China
share_percent: 37.3
year: 2025
- country: Chile
share_percent: 16.2
year: 2025
- country: United States
share_percent: 15.4
year: 2025
- country: Peru
share_percent: 15
year: 2025
- country: Mexico
share_percent: 6.5
year: 2025
critical_lists: []
recycling: 'USGS 2026: molybdenum is recycled as a component of catalysts, ferrous scrap and superalloy scrap.'
substitutes:
- 'USGS 2026: little substitution for molybdenum in steels and cast irons. Potential substitutes in alloy steels include boron, chromium, niobium and vanadium, and tungsten in tool steels.'
source: usgs-mcs2026-molybdenum
where: World Mine Production and Reserves table, 2025e column (world total 260,000 t). Shares calculated by this file from the printed tonnage over that total. Recycling and Substitutes paragraphs. Abundance from USGS PP 1802-A Table A1.
media: []
documents:
- title: Stanford Advanced Materials, Safety data sheet, Molybdenum carbide (CAS 12069-89-5), revision 3, 30-Mar-2024
type: sds
url: https://www.samaterials.com/tds/sc/1752570513-ST0225.pdf
year: 2024
- title: SAMaterials, Micro molybdenum carbide (Mo2C) powder, product page
type: datasheet
url: https://samaterials.com/micro-nano-materials/201-micro-molybdenum-carbide.html
- title: Nanografi, Molybdenum carbide (Mo2C) micron powder, purity 99.5, size 2.6 µm, hexagonal, product page
type: datasheet
url: https://shop.nanografi.com/microparticles/molybdenum-carbide-mo2c-micron-powder-purity-99-5-size-2-6-m-hexagonal/
- title: Hussain, Vikraman, Feroze, Song, An, Kim, Chun and Jung, Synthesis of Mo2C and W2C nanoparticle electrocatalysts for the efficient hydrogen evolution reaction in alkali and acid electrolytes, Frontiers in Chemistry 7:716 (2019)
type: paper
url: https://www.frontiersin.org/articles/10.3389/fchem.2019.00716/pdf
year: 2019
- title: Darujati, thesis on the effect of reforming gases on molybdenum carbide oxidation, Washington State University (2002)
type: report
url: https://rex.libraries.wsu.edu/esploro/outputs/graduate/The-effect-of-reforming-gases-on/99900525277201842
year: 2002
- title: Likith et al., Thermodynamic stability of molybdenum oxycarbides formed from orthorhombic Mo2C in oxygen-rich environments, J. Phys. Chem. C 122(2), 1223-1233 (2018), arXiv:1803.11546
type: paper
url: https://arxiv.org/abs/1803.11546
year: 2018
- title: USGS Mineral Commodity Summaries 2026, Molybdenum
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-molybdenum.pdf
year: 2026
- title: USGS Professional Paper 1802-A, Critical Mineral Resources of the United States, Table A1 (crustal abundances)
type: report
url: https://pubs.usgs.gov/pp/1802/a/pp1802a.pdf
year: 2017
- title: NIST Atomic Weights and Isotopic Compositions, molybdenum (atomic number 42, standard atomic weight 95.95(1))
type: database
url: https://physics.nist.gov/cgi-bin/Compositions/stand_alone.pl?ele=Mo&all=all&ascii=html
- title: NIST Atomic Weights and Isotopic Compositions, carbon (atomic number 6, standard atomic weight printed as [12.0096, 12.0116])
type: database
url: https://physics.nist.gov/cgi-bin/Compositions/stand_alone.pl?ele=C&all=all&ascii=html
- title: Wikipedia, Molybdenum carbide (composition, phases and history only)
type: database
url: https://en.wikipedia.org/wiki/Molybdenum_carbide
gaps:
- 'Hardness of pure Mo2C: no measured value read. The only Mo-based coating values found were for Mo2BC and Mo-B-C films, which are different phases, so they are not used. Wikipedia gives no hardness figure.'
- 'Thermal conductivity, coefficient of thermal expansion and elastic modulus of monolithic Mo2C: no fetched source with a printed value. The Mo2C-SiC co-sputtering paper (EPJ Applied Physics 2016) returned HTTP 403, so its values were not read.'
- 'MoC (the gamma phase): no MoC-specific property was read from a fetched source. Wikipedia names the composition and says the gamma phase has the same structure as tungsten carbide, which is composition and history only and is not used as a property.'
- Density and melting point rely on vendor pages and one SDS only. The Wikipedia infobox prints 8.90 g/cm3 and 2687 °C; the brief allows Wikipedia for composition and history only, so the 8.90 density is not used. PubChem returned a browser check and gave no value.
- 'Designations (UNS, EN, DIN, JIS, ASTM and similar): no fetched source printed a designation for this material. None are listed.'
- 'Catalysis use: the 2010 AIChE abstract on Pt/Mo2C catalysts returned HTTP 403. The catalysis claim here (alkane isomerisation) is a vendor statement only. No hydrotreating, CO2 hydrogenation or Levy and Boudart source was read.'
- 'Hard-coating use: no fetched source gives a Mo2C coating result with a number. The vendor page calls the powder a wear-resistant material with no test data.'
- 'Air oxidation of Mo2C powder: no onset temperature or mass gain in air was found in a source read in this run. The 600 °C onset is for steam and CO2 only.'
- 'Production route (carburisation or carbothermal reduction): no fetched source. Carbon feedstock is therefore not recorded beyond the formula.'
- 'Critical-mineral status of molybdenum (USGS 2025 critical list, EU critical raw materials list): not read in this run, so critical_lists is empty. The USGS MCS 2026 molybdenum PDF text read in this run does not mention the critical list.'
- 'Molybdenum crustal abundance: no molybdenum row in USGS PP 1802-A Table A1 (carbon is listed at 200 ppm in that table).'
- 'Environments: no source read supports a space environment tag, so tags.environments is empty.'
- 'Hazards: only the SAMaterials SDS was read. American Elements (page returned 404) and other supplier SDS pages were searched but not read. No GHS hazard statement was found for Mo2C in a fetched page.'
- 'Property names not in property-canon.yaml: tafel_slope, exchange_current_density, turnover_frequency and particle_size. Values are kept in the units the authors print.'
- The two density values (9.18 and 9.20 g/cm3) and the two melting values (2687 and 2690 °C) differ between vendors. Both are kept; no single value is chosen.
- The two HER overpotentials (-134 mV in 0.5 M H2SO4 and -116 mV in 1 M KOH, Hussain et al. 2019 Table 1) are printed with a Unicode minus sign, so the value check cannot match them. They are kept in the uses and story text, and removed from properties until the check reads that glyph.
- 'Atomic weight of molybdenum: NIST prints 95.95(1), and 95.95 is used with the parenthesised uncertainty dropped. Carbon is printed as an interval, [12.0096, 12.0116]; the lower bound is used in the recipe.'
sources:
sam-mo2c-sds:
title: Stanford Advanced Materials, Safety data sheet, Molybdenum carbide, revision 3 (30-Mar-2024)
url: https://www.samaterials.com/tds/sc/1752570513-ST0225.pdf
kind: datasheet
license: supplier safety data sheet, cited not reproduced
sam-mo2c-product:
title: SAMaterials, Micro molybdenum carbide (Mo2C) powder, product page
url: https://samaterials.com/micro-nano-materials/201-micro-molybdenum-carbide.html
kind: datasheet
license: vendor product page, cited not reproduced
nanografi-mo2c:
title: Nanografi, Molybdenum carbide (Mo2C) micron powder, product page
url: https://shop.nanografi.com/microparticles/molybdenum-carbide-mo2c-micron-powder-purity-99-5-size-2-6-m-hexagonal/
kind: datasheet
license: vendor product page, cited not reproduced
hussain-2019:
title: Hussain et al., Synthesis of Mo2C and W2C nanoparticle electrocatalysts for the efficient hydrogen evolution reaction in alkali and acid electrolytes, Frontiers in Chemistry 7:716 (2019)
url: https://www.frontiersin.org/articles/10.3389/fchem.2019.00716/pdf
kind: paper
license: open access, cited not reproduced
darujati-2002:
title: Darujati, Washington State University thesis (2002), effect of reforming gases on molybdenum carbide oxidation
url: https://rex.libraries.wsu.edu/esploro/outputs/graduate/The-effect-of-reforming-gases-on/99900525277201842
kind: report
license: university repository, cited not reproduced
likith-2018:
title: Likith et al., Thermodynamic stability of molybdenum oxycarbides formed from orthorhombic Mo2C in oxygen-rich environments, J. Phys. Chem. C 122(2) (2018), arXiv:1803.11546
url: https://arxiv.org/abs/1803.11546
kind: paper
license: arXiv preprint, cited not reproduced
usgs-mcs2026-molybdenum:
title: USGS Mineral Commodity Summaries 2026, Molybdenum
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-molybdenum.pdf
kind: report
license: public domain (USGS)
usgs-pp1802a:
title: USGS Professional Paper 1802-A, Critical Mineral Resources of the United States, Table A1 (crustal abundances)
url: https://pubs.usgs.gov/pp/1802/a/pp1802a.pdf
kind: report
license: public domain (USGS)
nist-mo:
title: NIST, Atomic weights and isotopic compositions for all elements, molybdenum
url: https://physics.nist.gov/cgi-bin/Compositions/stand_alone.pl?ele=Mo&all=all&ascii=html
kind: database
license: NIST public data
nist-c:
title: NIST, Atomic weights and isotopic compositions for all elements, carbon
url: https://physics.nist.gov/cgi-bin/Compositions/stand_alone.pl?ele=C&all=all&ascii=html
kind: database
license: NIST public data
wikipedia-mo2c:
title: Wikipedia, Molybdenum carbide (composition, phases and history only)
url: https://en.wikipedia.org/wiki/Molybdenum_carbide
kind: web
license: CC-BY-SA 4.0
license: CC-BY-4.0
updated: '2026-10-26'
review:
status: draft
method: assistant
checked_values: 11
unreachable: 3
caveats: 6
note: 'Written in this run from pages read in this run: the SAMaterials SDS (revision 30-Mar-2024), the SAMaterials product page, the Nanografi product page, Hussain et al. 2019 Table 1 and the TOF paragraph, the Darujati 2002 WSU abstract, the Likith et al. 2018 arXiv abstract, the USGS MCS 2026 molybdenum PDF, the USGS PP 1802-A PDF, NIST atomic weights for Mo and C, and Wikipedia for composition and history only. Unreachable: PubChem (browser check), AIChE 2010 abstract (HTTP 403), EPJ Applied Physics 2016 abstract (HTTP 403).'
story:
recipe:
line: Mo2C is a molybdenum-carbon compound with two molybdenum atoms and one carbon atom per formula unit. Wikipedia lists MoC and Mo2C as the two compositions of this system, with at least three phases. The synthesis route is not sourced in this file.
parts:
- name: Molybdenum
symbol: Mo
atoms: 2
atomic_weight: 95.95
role: The metal sublattice. The NIST standard atomic weight is 95.95 with an uncertainty of 1 in the last digit.
- name: Carbon
symbol: C
atoms: 1
atomic_weight: 12.0096
role: Sits in the interstitial sites of the metal lattice. NIST prints the standard atomic weight as the interval 12.0096 to 12.0116, and the lower bound is used.
risk_groups:
- title: For people
level: 0
verdict: Not classed hazardous, but dust must be kept down
lead: The supplier SDS classes the powder as not hazardous under OSHA 2012, but the toxicology has not been fully investigated. Treat the dust as the main handling concern.
points:
- label: Dust
line: The SDS says to avoid dust formation. It lists an ACGIH TLV of 10 mg/m3 as a TWA.
- label: Toxicology
line: The SDS states that the toxicological properties have not been fully investigated, and gives no irritation or sensitization data.
- title: If the powder heats in steam or CO2
lead: These numbers come from the Darujati thesis on Mo2C oxidation in steam and CO2.
points:
- label: Onset
line: Oxidation starts at about 600 °C in either steam or CO2. Above 750 °C the paper describes decomposition and then oxidation of the Mo metal.
why: Molybdenum carbide is a dense, high-melting carbide with two sourced uses. A vendor describes the powder as a superhard tool material and a wear-resistant material, with no test data. Hussain et al. (2019) show that chemically reduced Mo2C nanoparticles on nickel foam are an active, noble-metal-free electrocatalyst for hydrogen evolution in both acid and alkaline water. Its composition and phase names come from Wikipedia, which is used for composition and history only.
uses:
- where: Wear and tool materials
line: A vendor page lists Mo2C powder as a superhard tool material and a wear-resistant material. The page gives no test numbers.
- where: Hydrogen-evolution electrocatalyst
line: In 0.5 M H2SO4 the Mo2C catalyst reaches 10 mA cm-2 at -134 mV, with a Tafel slope of 83 mV dec-1. In 1 M KOH it reaches the same current density at -116 mV, with a Tafel slope of 65 mV dec-1 (Hussain et al. 2019).
- where: Catalysis in general
line: A vendor page says Mo2C is used as a catalyst for reactions involving hydrogen, such as alkane isomerisation. No primary source for this use was read in this run.
can_do:
- label: Melting
benchmark: melting_point
line: The SDS gives a melting point of 2687 °C. The Nanografi micron powder is listed at 2690 °C. The two are kept side by side.
- label: Density
benchmark: density
line: Two vendors list 9.18 g/cm3 and 9.20 g/cm3. No measurement method is given by either vendor.
- label: Hydrogen evolution
benchmark: tafel_slope
line: At 10 mA cm-2 the overpotential is -134 mV in 0.5 M H2SO4 and -116 mV in 1 M KOH, with the catalyst on nickel foam (Hussain et al. 2019). These depend on electrolyte and substrate.
compare: The Mo2C densities from two vendors (9.18 and 9.20 g/cm3) are higher than the density of titanium carbide in its own profile, and the Mo2C melting point (2687 °C in the SDS) is also high for a carbide. The HER overpotential is only meaningful against other catalysts in the same electrolyte and on the same substrate, so no cross-catalyst ranking is made here. Molybdenum diboride (MoB2) is a related molybdenum boride, mentioned here for context only and not profiled in this file.
compare_rows:
- label: Density
benchmark: density
- label: Melting point
benchmark: melting_point
- label: Tafel slope in 0.5 M H2SO4
benchmark: tafel_slope
handling:
- 'Dust: keep the powder from dispersing. The SDS says to avoid dust formation.'
- 'Oxidants: keep away from oxidising agents, which the SDS lists as incompatible.'
- 'Heat: in steam or CO2 the carbide oxidises from about 600 °C, so plan for oxide formation in hot service.'
good_for:
- Hard, high-melting powder for wear parts and tool materials, as claimed by the vendor. No test data are sourced here.
- Noble-metal-free electrocatalysis for hydrogen evolution in acid and alkaline water, per Hussain et al. 2019.
watch_out:
- Oxidation in steam or CO2 from about 600 °C, and oxycarbide formation under oxygen-bearing conditions (Likith et al. 2018).
- The SDS does not fully investigate toxicology, and the dust must be kept down even though the powder is not classed as hazardous.
- China imposed export controls on molybdenum powders in February 2025 (USGS MCS 2026). This affects supply of the feedstock, not the Mo2C itself.
- Hardness, thermal conductivity and expansion of pure Mo2C are not settled here.
verdict: Molybdenum carbide is a high-melting, dense carbide with a sourced hydrogen-evolution record and a vendor-stated use as a tool and wear material. Its hardness, thermal properties and air oxidation kinetics are not sourced in this file. The powder is classed as not hazardous, but its toxicology is not fully investigated and it oxidises from about 600 °C in steam or CO2.
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.