Rose's metal, Newton's metal, Field's metal and the bismuth-lead and bismuth-tin eutectics -
Rose's metal and Newton's metal are bismuth-lead-tin alloys (Rose's nominal 50 Bi, 25 Pb, 25 Sn by mass
This profile covers a family of bismuth-based fusible alloys that melt well below 150 °C.
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Melt low
98 °C melting point
Melt lower
62 °C melting point
Weight
10.44 g/cm3 density
Strength
44.1 MPa tensile
Recipe, share of the weight
- Bi 50%Bismuth
- Pb 25%Lead
- Sn 25%Tin
Best for
Low-temperature fusible releases and heat-transfer baths. Rose's metal is used as a heat-transfer medium in heating baths, and Newton's metal was proposed as easily shaped radiotherapy shielding
Weakest at
Field's metal is costly because indium is expensive. Lead-bearing alloys carry lead toxicity, and few physical or corrosion data were found for the solid alloys
Risk at a glance
- People Moderate. Lead and indium compounds are toxic
- If it fails High. Exposure to lead from fume or dust
- Corrosion No data. No corrosion data recorded
Quick facts: -
| Property | Value | Basis |
|---|---|---|
| Density | 8.56 to 10.4 g/cm³ | 2 sourced values across conditions |
| Tensile strength | 44.1 MPa | 1 sourced value |
| Thermal conductivity | 4 W/(m·K) | 1 sourced value |
| Melting point | 94 to 138 °C | 6 sourced values across conditions |
| Specific heat | 155 J/(kg·K) | 1 sourced value |
| Electrical resistivity | 4.3e-7 Ω·m | 1 sourced value |
What is the density of Rose's metal, Newton's metal, Field's metal (-)?
Rose's metal, Newton's metal, Field's metal (-) has a density of 8.56 to 10.4 g/cm³. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the thermal conductivity of Rose's metal, Newton's metal, Field's metal (-)?
Rose's metal, Newton's metal, Field's metal (-) has a thermal conductivity of 4 W/(m·K). The source and test conditions are listed in the properties table on this page.
What is the melting point of Rose's metal, Newton's metal, Field's metal (-)?
Rose's metal, Newton's metal, Field's metal (-) has a melting point of 94 to 138 °C. The range covers 6 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the tensile strength of Rose's metal, Newton's metal, Field's metal (-)?
Rose's metal, Newton's metal, Field's metal (-) has a tensile strength of 44.1 MPa. The source and test conditions are listed in the properties table on this page.
What is Rose's metal, Newton's metal, Field's metal (-) used for?
Uses recorded in the sources include Heat-transfer medium in heating baths; Easily shaped shielding for radiotherapy; Low-temperature solder (bismuth-tin eutectic).
Why it exists
Rose's metal is a low-melting alloy of bismuth, lead and tin, and Newton's metal is a close relative. Their melting points are low enough for heat-transfer baths and fusible releases. Field's metal trades a lead-free composition for a lower melting point (about 62 °C) and a high cost, since indium is expensive. The bismuth-lead eutectic is the coolant alloy in the OECD-NEA review, and the bismuth-tin eutectic is listed in the AIM solder table. Wikipedia gives the history of Rose's metal: the German chemist Valentin Rose the Elder discovered it.
Where it's used
Heat-transfer baths
Wikipedia says Rose's metal is used as a heat-transfer medium in heating baths. It is also used as a solder, to set cast iron railings in stone, and as a filler that keeps tubes from crimping while they are bent.
Radiation treatment shielding
Wikipedia says Newton's metal is comparable to Cerrobend without Cerrobend's cadmium, which has encouraged its use for easily shaped shielding in radiotherapy. This is a ground medical use.
Low-temperature solder
The AIM Solder alloy sheet lists the bismuth-tin eutectic, Bi58 with 138 °C melting point, among its specialty solder alloys. Wikipedia notes the alloy has reasonable shear strength and fatigue properties.
Recipe
Rose's metal and Newton's metal are bismuth-lead-tin alloys (Rose's nominal 50 Bi, 25 Pb, 25 Sn by mass; Newton's 50.0 Bi, 31.2 Pb, 18.8 Sn). Field's metal is a bismuth-indium-tin eutectic (32.5 Bi, 51 In, 16.5 Sn). The bismuth-lead eutectic is 55.5 Bi with 44.5 Pb, and the bismuth-tin eutectic is 58 Bi with 42 Sn. All are alloys, not compounds.
Rose's metal is a bismuth-lead-tin alloy, not a eutectic, with nominal composition 50% bismuth, 25% lead and 25% tin by mass (Wikipedia table). The article gives a wider range of 25 to 28% lead and 22 to 25% tin. The sources read do not describe how the alloy is made.
| Ingredient | Share of the weight | What it does |
|---|---|---|
| Bismuth Bi | 50% | The largest share. It makes up half the alloy and gives it a low melting point. Wikipedia describes elemental bismuth as having unusually low toxicity for a heavy metal. |
| Lead Pb | 25% | A heavy, soft component. Its share is 25 to 28% in the article text. Lead is the reason for most of the toxicity warnings in this profile. |
| Tin Sn | 25% | A component that adds to the low melting point. The article gives 22 to 25% tin. |
Weight shares are as printed in the sources.
What it can do
Melt low
98 °C melting point
measured
Rose's metal melts at 98 °C in the Wikipedia table and between 94 and 98 °C in its article. Newton's metal melts at 97 °C.
Melt lower
62 °C melting point
measured
Field's metal, the bismuth-indium-tin eutectic, becomes liquid at about 62 °C (144 °F).
Weight
10.44 g/cm3 density
measured
The bismuth-lead eutectic has a density of 10.44 g/cm3 on a supplier page. The bismuth-tin eutectic is 8.56 g/cm3 on another supplier page. No density is recorded for Rose's metal.
Strength
44.1 MPa tensile
measured
The bismuth-lead eutectic has a tensile strength of 44.1 MPa on a supplier page, without a test method. It stretches 37.5% before it breaks.
How it compares
These alloys sit at the low-melting end of the metal family. Rose's metal and Newton's metal melt at 97 to 98 °C, 27 to 28 °C above Wood's metal (70 °C in the Wikipedia table), and both carry lead rather than cadmium. Field's metal, at about 62 °C, is the lowest of the group, but it is an indium alloy and costs more. The bismuth-lead eutectic at 124 °C and the bismuth-tin eutectic at 138 °C sit above Rose's metal. For the values that exist, the bismuth-lead eutectic is the most complete record.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | - | Sn | Pb | Bi | In | Cd | Sb | Pb-Sb | SnPb | SAC305 | - | GaInSn | In-Sn / In-Ag | SnZn and SnBi | Sn-Sb-Cu | Pb alloys |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Thermal behavior and safety | ||||||||||||||||
| Melting point, Rose's metal (50 Bi, 25 Pb, 25 Sn) | 98 °C1 | 231.9 °C | 327.5 °C | 271.3 °C | 156.6 °C | 321 °C | 630.7 °C | 630 °C | 183 °C | 217 °C | 70 °C | -19 °C | 118 °C | 199 °C | 241 to 354 °C | 179 °C |
| Melting range, Rose's metal (article text) | 94 to 98 °C2 | 231.9 °C | 327.5 °C | 271.3 °C | 156.6 °C | 321 °C | 630.7 °C | 630 °C | 183 °C | 217 °C | 70 °C | -19 °C | 118 °C | 199 °C | 241 to 354 °C | 179 °C |
| Melting point, Newton's metal (Bi 50.0, Pb 31.2, Sn 18.8) | 97 °C3 | 231.9 °C | 327.5 °C | 271.3 °C | 156.6 °C | 321 °C | 630.7 °C | 630 °C | 183 °C | 217 °C | 70 °C | -19 °C | 118 °C | 199 °C | 241 to 354 °C | 179 °C |
| Melting point, Field's metal (32.5 Bi, 51 In, 16.5 Sn) | 62 °C4 | 231.9 °C | 327.5 °C | 271.3 °C | 156.6 °C | 321 °C | 630.7 °C | 630 °C | 183 °C | 217 °C | 70 °C | -19 °C | 118 °C | 199 °C | 241 to 354 °C | 179 °C |
| Melting point, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | 124 °C5 | 231.9 °C | 327.5 °C | 271.3 °C | 156.6 °C | 321 °C | 630.7 °C | 630 °C | 183 °C | 217 °C | 70 °C | -19 °C | 118 °C | 199 °C | 241 to 354 °C | 179 °C |
| Eutectic melting point, bismuth-lead (55.5 wt% Bi) | 124 °C6 | 231.9 °C | 327.5 °C | 271.3 °C | 156.6 °C | 321 °C | 630.7 °C | 630 °C | 183 °C | 217 °C | 70 °C | -19 °C | 118 °C | 199 °C | 241 to 354 °C | 179 °C |
| Specific heat, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | 155 J/kg-K11 | 213 J/(kg·K) | no data | no data | 234 J/(kg·K) | no data | 205 J/(kg·K) | no data | no data | no data | no data | no data | no data | 0.239 J/g-°C | no data | no data |
| Thermal conductivity, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | 4 W/m-K12 | 66.8 W/(m·K) | 35 W/(m.K) | 8 W/(m·K) | 81.8 W/(m·K) | 97 W/(m·K) | 24.4 W/(m·K) | no data | 49 W/m·K | 61 W/mK | no data | 25.4 W/m.K | 34 W/m·K | 61 W/m-K | no data | 49 W/m·K |
| Eutectic melting point, bismuth-tin (Bi 58, Sn 42) | 138 °C13 | 231.9 °C | 327.5 °C | 271.3 °C | 156.6 °C | 321 °C | 630.7 °C | 630 °C | 183 °C | 217 °C | 70 °C | -19 °C | 118 °C | 199 °C | 241 to 354 °C | 179 °C |
| Physical and electrical | ||||||||||||||||
| Density, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | 10.44 g/cm³7 | 7310 kg/m3 | 11.34 g/cm³ | 9.78 g/cm³ | 7.31 g/cm³ | 8.69 g/cm³ | 6.68 g/cm³ | 6.68 g/cm³ | 8.4 g/cm³ | 7.35 g/cc | 10.15 g/cm³ | 6.44 g/cm³ | 7.3 g/cm³ | 7.27 g/cc | 7.39 g/cm³ | 11.28 - |
| Electrical resistivity, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | 43 µOhmcm10 | 12.6 µΩ·cm | 2.1×10^-7 ohm.m | 130 µΩ·cm | 8.8 µΩ·cm | no data | 40.1 µΩ·cm | no data | 1.45×10^-5 ohm-cm | 13.2 μ Ohm-cm | no data | no data | 0.147 µΩ·m | 1.1×10^-5 ohm-cm | no data | 1.45×10^-5 ohm-cm |
| Density, bismuth-tin (Bi 58, Sn 42) | 8.56 g/cm³14 | 7310 kg/m3 | 11.34 g/cm³ | 9.78 g/cm³ | 7.31 g/cm³ | 8.69 g/cm³ | 6.68 g/cm³ | 6.68 g/cm³ | 8.4 g/cm³ | 7.35 g/cc | 10.15 g/cm³ | 6.44 g/cm³ | 7.3 g/cm³ | 7.27 g/cc | 7.39 g/cm³ | 11.28 - |
| Other measurements | ||||||||||||||||
| Tensile strength, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | 44.1 MPa8 | no data | no data | no data | 2.6 to 4.5 MPa | no data | no data | 34.8 to 38.9 MPa | 43 MPa | 39.58 MPa | no data | no data | 12 MPa | 54.7 MPa | 77 MPa | 43 MPa |
| Elongation at break, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | 37.5 %9 | no data | no data | no data | no data | no data | no data | 7.2 to 8.2 % | 40 % | 49 % | no data | no data | no data | 32.5 % | 18 % | 40 % |
Why choose it, and why not
Good for
- Heat-transfer baths held near 98 °C, where Rose's metal is used (Wikipedia).
- Fusible releases near 62 °C, where Field's metal is used as a low-melting, lead-free option (Wikipedia).
Watch out for
- Lead: Rose's, Newton's and the bismuth-lead eutectic contain lead, and PubChem records H360FD and H362 for lead.
- Indium cost: Field's metal is costly, since its major component is indium, which Wikipedia says costs about double the price of silver.
- Few physical data: no density for Rose's metal, and no thermal or tensile data for Rose's, Newton's or Field's metal in any source read.
Rose's metal and Newton's metal are lead-containing fusible alloys that melt at 97 to 98 °C. Field's metal is a lead-free, indium-based alternative at 62 °C. The bismuth-lead and bismuth-tin eutectics have the most complete data. The physical data for the three named alloys are thin, and lead's toxicity is the main hazard.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Melting point, Rose's metal (50 Bi, 25 Pb, 25 Sn) | Value in the well-known alloys table of an encyclopedia article (secondary source; underlying measurement not named) | composition 50 % Bi, 25 % Pb, 25 % Sn by mass (the composition the table prints)basis eutectic flag printed as No; the article text gives a range (see the next row) | — |
| 2 | Melting range, Rose's metal (article text) | Stated in the lead section of an encyclopedia article (secondary source; underlying measurement not named) | composition 50 % Bi, 25 to 28 % Pb, 22 to 25 % Sn by mass (the article text range) | The article text gives the wider composition range; the table uses the 50/25/25 composition, which gives 98 °C. |
| 3 | Melting point, Newton's metal (Bi 50.0, Pb 31.2, Sn 18.8) | Stated in the lead section of an encyclopedia article (secondary source) | composition 8 parts Bi, 5 parts Pb, 3 parts Sn by weight (the article); Bi 50.0, Pb 31.2, Sn 18.8 in the table | — |
| 4 | Melting point, Field's metal (32.5 Bi, 51 In, 16.5 Sn) | Stated in the lead section of an encyclopedia article (secondary source) | composition 32.5 % Bi, 51 % In, 16.5 % Sn by massbasis stated as approximately 62 °C (144 °F) | The Wikipedia table prints 62 °C (144 °F) and marks the alloy as eutectic. Field's metal contains indium, not lead. |
| 5 | Melting point, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | Value printed on a supplier product page for the 55.5/44.5 eutectic | composition 55.5 Bi, 44.5 Pb by weight (eutectic) | The Wikipedia Other alloys table prints 125 °C for the same composition and an OECD-NEA review passage prints 123.5 °C. The OECD review also gives 124 °C (397 K) in its phase-diagram text, and the value in this row is the supplier's. |
| 6 | Eutectic melting point, bismuth-lead (55.5 wt% Bi) | Value stated in the phase-diagram description of an OECD-NEA review chapter on lead-bismuth thermophysical properties | composition 55.5 wt% Bi, 44.5 wt% Pb (eutectic) | The same chapter quotes the eutectic as 124 C (397 K) in its diagram text; it also records a historical value of 123.5 C for the 55.5 % Bi eutectic in its text. |
| 7 | Density, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | Value printed on a supplier product page in the physical properties table | composition Bi 55.5 / Pb 44.5temperature not stated on the page | — |
| 8 | Tensile strength, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | Value printed on a supplier product page in the mechanical properties table | composition Bi 55.5 / Pb 44.5test method not stated on the pageproduct form not stated on the page | The supplier prints no test method or form, so treat the value as indicative. The source does not give a temperature. |
| 9 | Elongation at break, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | Value printed on a supplier product page in the mechanical properties table | composition Bi 55.5 / Pb 44.5test method not stated on the page | — |
| 10 | Electrical resistivity, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | Value printed on a supplier product page, copied with the unit as printed (µOhmcm) | composition Bi 55.5 / Pb 44.5temperature not stated on the page | — |
| 11 | Specific heat, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | Value printed on a supplier product page; the page prints the unit as J K-1 kg-1 | composition Bi 55.5 / Pb 44.5temperature 23 °C | — |
| 12 | Thermal conductivity, bismuth-lead eutectic (Bi 55.5, Pb 44.5) | Value printed on a supplier product page; the page prints the unit as W m-1 K-1 | composition Bi 55.5 / Pb 44.5temperature 85 °C | — |
| 13 | Eutectic melting point, bismuth-tin (Bi 58, Sn 42) | Value printed on the AIM Solder alloy information sheet, specialty solder table | composition Bi 58 / Sn 42 (eutectic) | — |
| 14 | Density, bismuth-tin (Bi 58, Sn 42) | Value printed on a supplier product page in the physical properties table | composition Bi 58 / Sn 42temperature not stated on the page | The AIM sheet prints the density in pounds per cubic inch (.3090) and is not converted here. |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Molten bismuth-lead eutectic as a liquid-metal coolant (nuclear reactor and accelerator-driven systems) | not rated | The OECD-NEA review expects the low melting point to give lower corrosion rates, but it quotes no number.1 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Molten bismuth-lead eutectic as a liquid-metal coolant (nuclear reactor and accelerator-driven systems) | The review says that LBE's low melting temperature of about 397 K (about 124 °C) results in lower corrosion rates and in easier maintenance. It gives no corrosion figure, and the statement applies to the molten alloy in a reactor, not to solid parts. | basis Qualitative statement in the introduction of a thermophysical-properties chapter; no test condition is givencomposition Bi 55.5 wt% / Pb 44.5 wt% (LBE) |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
The alloys that contain lead carry lead's hazard codes. Field's metal contains indium, whose compounds are toxic when inhaled, according to Wikipedia.
- Lead
- PubChem's ECHA aggregate for lead reports H360FD, H362, H400 and H410, with signal word Danger. Wikipedia says lead is poisonous whether inhaled or swallowed.
- Indium
- PubChem's indium record lists H302, H312, H315, H319, H332, H335 and H372 with signal word Danger. Field's metal is about 51% indium.
- Bismuth
- Wikipedia says elemental bismuth has unusually low toxicity for a heavy metal. PubChem's bismuth record has no GHS classification, with 324 of 382 company reports not meeting GHS criteria.
If it overheats
These alloys melt well below 150 °C, so a part in service can lose its shape or release its load above the melting point.
- Rose's metal
- The alloy melts between 94 and 98 °C (article), and the Wikipedia table gives 98 °C for the 50/25/25 composition.
- Newton's metal
- Newton's metal melts at 97 °C.
- Field's metal
- Field's metal becomes liquid at about 62 °C (144 °F).
Handling and storage
- Lead-bearing alloys
- PubChem's lead record lists precautionary codes P260, P264, P270 and P280. Wikipedia says lead is toxic whether inhaled or swallowed. Dust and fume control is advice, not a figure from the sources.
- Solder mixing
- Wikipedia warns that combining the bismuth-tin eutectic with lead-tin solder may dramatically lower the melting point and lead to joint failure.
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Melting of Rose's metalmoderate severity | Temperature at or above about 94 to 98 °CThe alloy liquefies. This is the intended action for fusible plugs and for filling tubes that are bent after melting, but a part in service above that temperature loses its shape and load capacity. |
| Exposure to lead from fume or dusthigh severity | Melting or machining a lead-bearing alloy (Rose's, Newton's or bismuth-lead) without controlsLead is highly poisonous whether inhaled or swallowed, and PubChem's ECHA aggregate for lead reports reproductive-toxicity hazard codes. |
| Joint failure when bismuth-tin solder is mixed with lead-tin solderhigh severity | Combining the bismuth-rich eutectic with lead-tin solder in one jointWikipedia says the combination may dramatically lower the melting point and lead to joint failure. |
| Exposure to indium from heated or dusty Field's metalmoderate severity | Melting Field's metal or handling indium-rich dustIndium compounds are toxic when inhaled, according to Wikipedia. The liquid metal and the dust were not tested in any source read. |
Handling and storage
- PubChem's lead record lists precautionary codes P260, P264, P270 and P280 (the code text is not quoted here).
- Wikipedia says lead is toxic whether inhaled or swallowed, so do not melt, cut or grind lead-bearing alloys without ventilation and dust control.
Supply and geography
How common the raw materials are and where they come from.
Bismuth
USGS: bismuth is produced most often as a byproduct during the processing of lead ores.
- Top producers (2025)
- China 88%, Republic of Korea 6.3%
- Critical mineral lists
- US: listed
- Recycling
- USGS: recycled bismuth-containing alloy scrap was estimated to compose up to 10% of U.S. bismuth apparent consumption for 2021 to 2025.
- Substitutes
- USGS: cadmium, indium, lead and tin can partially replace bismuth in low-temperature solders; glycerin-filled glass bulbs can replace bismuth alloys in triggering devices for fire sprinklers.
Lead
- Top producers (2025)
- China 42.2%, Australia 10.7%, Peru 6.4%
- Critical mineral lists
- US: listed
- Recycling
- USGS: an estimated 1 million tons of secondary lead was produced in 2025, equivalent to 70% of apparent domestic consumption, mostly from lead-acid battery scrap.
- Substitutes
- USGS: plastics have reduced the use of lead in cable covering and cans, and steel and zinc are common substitutes for lead in wheel weights.
Tin
- Top producers (2025)
- China 24.5%, Indonesia 21%, Peru 11.4%
- Critical mineral lists
- US: listed
- Recycling
- USGS: about 17,000 tons of tin from old and new scrap was estimated to have been recycled in 2025, accounting for 22% of apparent consumption.
- Substitutes
- USGS: epoxy resins for solder are listed among materials that substitute for tin, and aluminum, glass, paper, plastic or tin-free steel substitute for tin in cans.
Indium
- Top producers (2025)
- China 70%
- Critical mineral lists
- US: listed
- Recycling
- USGS: indium is most commonly recovered from ITO scrap in Japan and the Republic of Korea.
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: roses-metal
spore_version: 0.2
family: low-melting-metals-and-solders
name: Rose's metal, Newton's metal, Field's metal and the bismuth-lead and bismuth-tin eutectics
abbreviation: '-'
role: low-melting fusible alloys (about 62 to 138 °C, bismuth-based)
category: metals
type: heavy-metals
summary: |
This profile covers a family of bismuth-based fusible alloys that melt well below 150 °C. Rose's metal is a bismuth-lead-tin alloy of nominal composition 50% bismuth, 25% lead and 25% tin by mass, with a melting point of 98 °C in the Wikipedia table and 94 to 98 °C in its article text. It was discovered by the German chemist Valentin Rose the Elder. Newton's metal (Bi 50.0, Pb 31.2, Sn 18.8) melts at 97 °C and was written about as a shielding material for radiotherapy. Field's metal is not a bismuth-lead or bismuth-tin alloy: it is a bismuth-indium-tin eutectic (32.5% Bi, 51% In, 16.5% Sn) that melts at about 62 °C, and it contains no lead or cadmium. The two binary eutectics are the bismuth-lead alloy 55.5% Bi with 44.5% Pb (melting at 124 °C in the OECD-NEA review and in a supplier page, and 125 °C in the Wikipedia table; the 45/55 figure in the brief is the same eutectic rounded), and the bismuth-tin alloy 58% Bi with 42% Sn at 138 °C. The bismuth-tin eutectic is listed in the AIM solder table and has a density of 8.56 g/cm3 on a Goodfellow page. Physical property data from a supplier exist only for the bismuth-lead eutectic (also in the OECD-NEA review) and the bismuth-tin eutectic. For Rose's metal, Newton's metal and Field's metal, only melting points and compositions were read; no density, thermal or tensile value could be read from an open page.
best_for: Low-temperature fusible releases and heat-transfer baths. Rose's metal is used as a heat-transfer medium in heating baths, and Newton's metal was proposed as easily shaped radiotherapy shielding
weakest_at: Field's metal is costly because indium is expensive. Lead-bearing alloys carry lead toxicity, and few physical or corrosion data were found for the solid alloys
identity:
formula: Rose's metal and Newton's metal are bismuth-lead-tin alloys (Rose's nominal 50 Bi, 25 Pb, 25 Sn by mass; Newton's 50.0 Bi, 31.2 Pb, 18.8 Sn). Field's metal is a bismuth-indium-tin eutectic (32.5 Bi, 51 In, 16.5 Sn). The bismuth-lead eutectic is 55.5 Bi with 44.5 Pb, and the bismuth-tin eutectic is 58 Bi with 42 Sn. All are alloys, not compounds.
source: wikipedia-fusible-alloy
where: Well-known alloys table (Rose's metal, Field's metal, Wood's metal rows) and Other alloys table (Newton's metal, Bi-Pb and Bi-Sn rows)
tags:
applications:
- thermal-control
- radiation-shielding
- electronics-and-chips
stresses: []
environments: []
properties:
- benchmark: melting_point
label: Melting point, Rose's metal (50 Bi, 25 Pb, 25 Sn)
value: 98
unit: °C
scope: material
conditions:
composition: 50 % Bi, 25 % Pb, 25 % Sn by mass (the composition the table prints)
basis: eutectic flag printed as No; the article text gives a range (see the next row)
method: Value in the well-known alloys table of an encyclopedia article (secondary source; underlying measurement not named)
status: ground
source: wikipedia-fusible-alloy
where: Well-known alloys table, Rose's metal row (98 °C (208 °F))
- benchmark: melting_point
label: Melting range, Rose's metal (article text)
value: 94
value_high: 98
bound: range
unit: °C
scope: material
conditions:
composition: 50 % Bi, 25 to 28 % Pb, 22 to 25 % Sn by mass (the article text range)
method: Stated in the lead section of an encyclopedia article (secondary source; underlying measurement not named)
status: ground
note: The article text gives the wider composition range; the table uses the 50/25/25 composition, which gives 98 °C.
source: wikipedia-roses-metal
where: 'Lead section: ''Its melting point is between 94 and 98 °C (201 and 208 °F)'''
- benchmark: melting_point
label: Melting point, Newton's metal (Bi 50.0, Pb 31.2, Sn 18.8)
value: 97
unit: °C
scope: material
conditions:
composition: 8 parts Bi, 5 parts Pb, 3 parts Sn by weight (the article); Bi 50.0, Pb 31.2, Sn 18.8 in the table
method: Stated in the lead section of an encyclopedia article (secondary source)
status: ground
source: wikipedia-newtons-metal
where: 'Lead section: ''its melting point is 97 °C'''
- benchmark: melting_point
label: Melting point, Field's metal (32.5 Bi, 51 In, 16.5 Sn)
value: 62
unit: °C
scope: material
conditions:
composition: 32.5 % Bi, 51 % In, 16.5 % Sn by mass
basis: stated as approximately 62 °C (144 °F)
method: Stated in the lead section of an encyclopedia article (secondary source)
status: ground
note: The Wikipedia table prints 62 °C (144 °F) and marks the alloy as eutectic. Field's metal contains indium, not lead.
source: wikipedia-fields-metal
where: 'Lead paragraph: ''becomes liquid at approximately 62 °C (144 °F)'''
- benchmark: melting_point
label: Melting point, bismuth-lead eutectic (Bi 55.5, Pb 44.5)
value: 124
unit: °C
scope: material
conditions:
composition: 55.5 Bi, 44.5 Pb by weight (eutectic)
method: Value printed on a supplier product page for the 55.5/44.5 eutectic
status: ground
note: The Wikipedia Other alloys table prints 125 °C for the same composition and an OECD-NEA review passage prints 123.5 °C. The OECD review also gives 124 °C (397 K) in its phase-diagram text, and the value in this row is the supplier's.
source: goodfellow-bipb
where: 'Thermal Properties table, Melting point ( C) row: 124'
- benchmark: melting_point
label: Eutectic melting point, bismuth-lead (55.5 wt% Bi)
value: 124
unit: °C
scope: material
conditions:
composition: 55.5 wt% Bi, 44.5 wt% Pb (eutectic)
method: Value stated in the phase-diagram description of an OECD-NEA review chapter on lead-bismuth thermophysical properties
status: ground
note: The same chapter quotes the eutectic as 124 C (397 K) in its diagram text; it also records a historical value of 123.5 C for the 55.5 % Bi eutectic in its text.
source: oecd-nea-lbe
where: 'Section 2.1 (Introduction) and the figure text on the bismuth-lead phase diagram: ''an eutectic point at 55.5 wt.% Bi with a melting temperature of 124C (397 K)'''
- benchmark: density
label: Density, bismuth-lead eutectic (Bi 55.5, Pb 44.5)
value: 10.44
unit: g/cm3
scope: material
conditions:
composition: Bi 55.5 / Pb 44.5
temperature: not stated on the page
method: Value printed on a supplier product page in the physical properties table
status: ground
source: goodfellow-bipb
where: Physical Properties table, Density row (10.44)
- benchmark: ultimate_tensile_strength
label: Tensile strength, bismuth-lead eutectic (Bi 55.5, Pb 44.5)
value: 44.1
unit: MPa
scope: material
conditions:
composition: Bi 55.5 / Pb 44.5
test_method: not stated on the page
product_form: not stated on the page
method: Value printed on a supplier product page in the mechanical properties table
status: ground
note: The supplier prints no test method or form, so treat the value as indicative. The source does not give a temperature.
source: goodfellow-bipb
where: Mechanical Properties table, Tensile strength (MPa) row (44.1)
- benchmark: elongation
label: Elongation at break, bismuth-lead eutectic (Bi 55.5, Pb 44.5)
value: 37.5
unit: '%'
scope: material
conditions:
composition: Bi 55.5 / Pb 44.5
test_method: not stated on the page
method: Value printed on a supplier product page in the mechanical properties table
status: ground
source: goodfellow-bipb
where: Mechanical Properties table, Elongation at break (%) row (37.5)
- benchmark: electrical_resistivity
label: Electrical resistivity, bismuth-lead eutectic (Bi 55.5, Pb 44.5)
value: 43
unit: µOhmcm
scope: material
conditions:
composition: Bi 55.5 / Pb 44.5
temperature: not stated on the page
method: Value printed on a supplier product page, copied with the unit as printed (µOhmcm)
status: ground
source: goodfellow-bipb
where: Electrical Properties table, Electrical resistivity row (43)
- benchmark: specific_heat
label: Specific heat, bismuth-lead eutectic (Bi 55.5, Pb 44.5)
value: 155
unit: J/kg-K
scope: material
conditions:
composition: Bi 55.5 / Pb 44.5
temperature: 23 °C
method: Value printed on a supplier product page; the page prints the unit as J K-1 kg-1
status: ground
source: goodfellow-bipb
where: Thermal Properties table, Specific heat row (155 at 23 °C)
- benchmark: thermal_conductivity
label: Thermal conductivity, bismuth-lead eutectic (Bi 55.5, Pb 44.5)
value: 4
unit: W/m-K
scope: material
conditions:
composition: Bi 55.5 / Pb 44.5
temperature: 85 °C
method: Value printed on a supplier product page; the page prints the unit as W m-1 K-1
status: ground
source: goodfellow-bipb
where: Thermal Properties table, Thermal conductivity row (4 at 85 °C)
- benchmark: melting_point
label: Eutectic melting point, bismuth-tin (Bi 58, Sn 42)
value: 138
unit: °C
scope: material
conditions:
composition: Bi 58 / Sn 42 (eutectic)
method: Value printed on the AIM Solder alloy information sheet, specialty solder table
status: ground
source: aim-alloy-information
where: Specialty solder alloys table, Bi58 row (58 Bi, 42 Sn, melting point 138 °C)
- benchmark: density
label: Density, bismuth-tin (Bi 58, Sn 42)
value: 8.56
unit: g/cm3
scope: material
conditions:
composition: Bi 58 / Sn 42
temperature: not stated on the page
method: Value printed on a supplier product page in the physical properties table
status: ground
note: The AIM sheet prints the density in pounds per cubic inch (.3090) and is not converted here.
source: goodfellow-bisn
where: Physical Properties table, Density (g cm-3) row (8.56)
corrosion:
- environment: Molten bismuth-lead eutectic as a liquid-metal coolant (nuclear reactor and accelerator-driven systems)
headline: The OECD-NEA review expects the low melting point to give lower corrosion rates, but it quotes no number.
effect: The review says that LBE's low melting temperature of about 397 K (about 124 °C) results in lower corrosion rates and in easier maintenance. It gives no corrosion figure, and the statement applies to the molten alloy in a reactor, not to solid parts.
rating: unknown
conditions:
basis: Qualitative statement in the introduction of a thermophysical-properties chapter; no test condition is given
composition: Bi 55.5 wt% / Pb 44.5 wt% (LBE)
source: oecd-nea-lbe
where: Section 2.1 (Introduction)
risks:
hazards:
- text: Wikipedia says lead is a highly poisonous metal, whether inhaled or swallowed, affecting almost every organ and system. Rose's metal, Newton's metal and the bismuth-lead eutectic all contain lead.
ghs: []
source: wikipedia-lead
where: Toxicity section
- text: 'PubChem reports ECHA notifications for elemental lead: H360FD (may damage fertility; may damage the unborn child), H362 (may cause harm to breast-fed children), H400 and H410 (very toxic to aquatic life), with signal word Danger. Reproductive toxicity category Repr. 1A is reported for 84.4% of company reports.'
ghs:
- H360FD
- H362
- H400
- H410
source: pubchem-lead
where: GHS Classification section, Hazard Statements and Regulation (EC) 1272/2008 classes (CID 5352425)
- text: 'PubChem reports for elemental indium: signal word Danger, with H302, H312, H315, H319, H332, H335 and H372 (H372 is reported for 63.3% of company reports). It also records that 69 of 371 company reports say the substance does not meet GHS criteria. Field''s metal contains about 51% indium by mass.'
ghs:
- H302
- H312
- H315
- H319
- H332
- H335
- H372
source: pubchem-indium
where: GHS Classification section, hazard statements with percentages (CID 5359967)
- text: Wikipedia says indium compounds are toxic when inhaled or injected into the bloodstream, although they are poorly absorbed after ingestion. It notes an overview that found no evidence of a health hazard from industrial use of indium.
ghs: []
source: wikipedia-indium
where: Occurrence and production (toxicity sentence in the introduction)
- text: 'Wikipedia says elemental bismuth has unusually low toxicity for a heavy metal. PubChem''s bismuth record has no GHS classification for the element: 324 of 382 company reports say it does not meet GHS criteria.'
ghs: []
source: pubchem-bismuth
where: Toxicology and GHS Classification sections (CID 5359367)
failure_risks:
- mode: Melting of Rose's metal
trigger: Temperature at or above about 94 to 98 °C
consequence: The alloy liquefies. This is the intended action for fusible plugs and for filling tubes that are bent after melting, but a part in service above that temperature loses its shape and load capacity.
severity: moderate
source: wikipedia-roses-metal
where: Lead section (melting range) and Uses section (tube filling)
- mode: Exposure to lead from fume or dust
trigger: Melting or machining a lead-bearing alloy (Rose's, Newton's or bismuth-lead) without controls
consequence: Lead is highly poisonous whether inhaled or swallowed, and PubChem's ECHA aggregate for lead reports reproductive-toxicity hazard codes.
severity: high
source: wikipedia-lead
where: Toxicity section; PubChem GHS Classification (CID 5352425)
- mode: Joint failure when bismuth-tin solder is mixed with lead-tin solder
trigger: Combining the bismuth-rich eutectic with lead-tin solder in one joint
consequence: Wikipedia says the combination may dramatically lower the melting point and lead to joint failure.
severity: high
source: wikipedia-fusible-alloy
where: Other alloys table, Bi58 note
- mode: Exposure to indium from heated or dusty Field's metal
trigger: Melting Field's metal or handling indium-rich dust
consequence: Indium compounds are toxic when inhaled, according to Wikipedia. The liquid metal and the dust were not tested in any source read.
severity: moderate
source: wikipedia-indium
where: Occurrence and production (toxicity sentence in the introduction)
side_effects: []
handling:
- text: PubChem's lead record lists precautionary codes P260, P264, P270 and P280 (the code text is not quoted here).
source: pubchem-lead
where: GHS Classification section, Precautionary Statement Codes
- text: Wikipedia says lead is toxic whether inhaled or swallowed, so do not melt, cut or grind lead-bearing alloys without ventilation and dust control.
source: wikipedia-lead
where: Toxicity section
mitigations: []
uses:
- application: thermal-control
device: Heat-transfer medium in heating baths
example: Wikipedia says Rose's metal is used as a heat-transfer medium in heating baths. This is a ground laboratory use.
source: wikipedia-roses-metal
where: Uses section, third use listed
- application: radiation-shielding
device: Easily shaped shielding for radiotherapy
example: Wikipedia says Newton's metal is comparable to Cerrobend without Cerrobend's cadmium, which has encouraged its use for easily shaped shielding during radiotherapy. This is a ground medical use, not a space use.
source: wikipedia-newtons-metal
where: Lead section, second and third sentences
- application: electronics-and-chips
device: Low-temperature solder (bismuth-tin eutectic)
example: The AIM Solder alloy sheet lists the Bi58 alloy, with melting point 138 °C, in its specialty solder table. The source does not describe a specific electronics use.
source: aim-alloy-information
where: Specialty solder alloys table, Bi58 row
supply:
- subject: Bismuth
producers:
- country: China
share_percent: 88
year: 2025
- country: Republic of Korea
share_percent: 6.3
year: 2025
critical_lists:
- list: USGS 2025 List of Critical Minerals
listed: true
recycling: 'USGS: recycled bismuth-containing alloy scrap was estimated to compose up to 10% of U.S. bismuth apparent consumption for 2021 to 2025.'
substitutes:
- 'USGS: cadmium, indium, lead and tin can partially replace bismuth in low-temperature solders; glycerin-filled glass bulbs can replace bismuth alloys in triggering devices for fire sprinklers.'
abundance: 'USGS: bismuth is produced most often as a byproduct during the processing of lead ores.'
source: usgs-mcs2026-bismuth
where: World Refinery Production table (2025; the China 88% share is printed in the Events paragraph; Republic of Korea 6.3% is 1,000 of 16,000 t, calculated by Space Mushroom); World Resources paragraph; Substitutes; critical list status from the USGS 2025 list page
- subject: Lead
producers:
- country: China
share_percent: 42.2
year: 2025
- country: Australia
share_percent: 10.7
year: 2025
- country: Peru
share_percent: 6.4
year: 2025
critical_lists:
- list: USGS 2025 List of Critical Minerals
listed: true
recycling: 'USGS: an estimated 1 million tons of secondary lead was produced in 2025, equivalent to 70% of apparent domestic consumption, mostly from lead-acid battery scrap.'
substitutes:
- 'USGS: plastics have reduced the use of lead in cable covering and cans, and steel and zinc are common substitutes for lead in wheel weights.'
source: usgs-mcs2026-lead
where: World Mine Production and Reserves table (2025e, thousand metric tons of lead content; world total 4,500; shares calculated by Space Mushroom from China 1,900, Australia 480 and Peru 290); Recycling; Substitutes; critical list status from the USGS 2025 list page
- subject: Tin
producers:
- country: China
share_percent: 24.5
year: 2025
- country: Indonesia
share_percent: 21
year: 2025
- country: Peru
share_percent: 11.4
year: 2025
critical_lists:
- list: USGS 2025 List of Critical Minerals
listed: true
recycling: 'USGS: about 17,000 tons of tin from old and new scrap was estimated to have been recycled in 2025, accounting for 22% of apparent consumption.'
substitutes:
- 'USGS: epoxy resins for solder are listed among materials that substitute for tin, and aluminum, glass, paper, plastic or tin-free steel substitute for tin in cans.'
source: usgs-mcs2026-tin
where: World Mine Production table (2025e, world total 290,000 t; shares calculated by Space Mushroom from China 71,000, Indonesia 61,000 and Peru 33,000); Recycling; Substitutes; critical list status from the USGS 2025 list page
- subject: Indium
producers:
- country: China
share_percent: 70
year: 2025
critical_lists:
- list: USGS 2025 List of Critical Minerals
listed: true
recycling: 'USGS: indium is most commonly recovered from ITO scrap in Japan and the Republic of Korea.'
substitutes: []
source: usgs-mcs2026-indium
where: Events paragraph (China accounts for 70% of the world total); Recycling; critical list status from the USGS 2025 list page. Import sources for 2021 to 2024 were Republic of Korea 25%, Japan 22%, China 12% and Canada 11%.
documents:
- title: 'Mineral Commodity Summaries 2026: Bismuth (USGS)'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-bismuth.pdf
year: 2026
- title: 'Mineral Commodity Summaries 2026: Lead (USGS)'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-lead.pdf
year: 2026
- title: 'Mineral Commodity Summaries 2026: Tin (USGS)'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-tin.pdf
year: 2026
- title: 'Mineral Commodity Summaries 2026: Indium (USGS)'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-indium.pdf
year: 2026
- title: About the 2025 List of Critical Minerals (USGS)
type: report
url: https://www.usgs.gov/programs/mineral-resources-program/science/about-2025-list-critical-minerals
year: 2025
- title: Fusible alloy (encyclopedia article, well-known alloys and other alloys tables)
type: database
url: https://en.wikipedia.org/wiki/Fusible_alloy
year: 2026
- title: Rose's metal (encyclopedia article)
type: database
url: https://en.wikipedia.org/wiki/Rose%27s_metal
year: 2026
- title: Field's metal (encyclopedia article)
type: database
url: https://en.wikipedia.org/wiki/Field%27s_metal
year: 2026
- title: Newton's metal (encyclopedia article)
type: database
url: https://en.wikipedia.org/wiki/Newton%27s_metal
year: 2026
- title: Bismuth (encyclopedia article)
type: database
url: https://en.wikipedia.org/wiki/Bismuth
year: 2026
- title: Lead (encyclopedia article, toxicity)
type: database
url: https://en.wikipedia.org/wiki/Lead
year: 2026
- title: Indium (encyclopedia article, occurrence and toxicity)
type: database
url: https://en.wikipedia.org/wiki/Indium
year: 2026
- title: Bismuth-lead alloy pellets, 55.5:44.5 eutectic (Goodfellow product page)
type: datasheet
url: https://www.goodfellow.com/usa/bismuth-lead-alloy-pellets-bi55-5-pb44-5-group
year: 2026
- title: Bismuth/tin alloy ingot, Bi58/Sn42 (Goodfellow product page)
type: datasheet
url: https://www.goodfellow.com:443/p/bi11-lp-000100/bismuth-tin-alloy-ingot
year: 2026
- title: Alloy information, common and specialty solder alloys (AIM Solder)
type: datasheet
url: https://aimsolder.com/wp-content/uploads/legacy-files/alloy_information.pdf
year: 2026
- title: 'Lead-bismuth eutectic: thermophysical and electric properties, chapter 2 (OECD-NEA, 2007)'
type: report
url: https://www.oecd-nea.org/science/reports/2007/pdf/chapter2.pdf
year: 2007
- title: 'PubChem compound record: Lead (CID 5352425), GHS classification'
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/5352425
year: 2026
- title: 'PubChem compound record: Indium (CID 5359967), GHS classification'
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/Indium
year: 2026
- title: 'PubChem compound record: Bismuth (CID 5359367), GHS classification'
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/Bismuth
year: 2026
gaps:
- 'Rose''s metal: no density, thermal conductivity, specific heat, tensile strength or elongation was read on an open page. The Thermo Fisher, Sigma-Aldrich and American Elements pages were blocked (HTTP 403 or no DNS), and the search snippets are not used as values.'
- 'Rose''s metal: the Thermo Fisher listing reports 95 to 96 °C and hazard statements, but its page could not be opened, so that value is not recorded.'
- 'Field''s metal: no density, thermal conductivity or tensile value was read. American Elements (density) and Fisher Scientific were blocked; university papers on its thermophysical properties were seen only as search results.'
- 'Field''s metal: a materials paper in search results gives a different melting temperature, which was not fetched, so the 62 °C value stands alone.'
- 'Newton''s metal: density, thermal and mechanical data were not found. The 2007 paper on Newton''s metal as shielding (Radiation Effects and Defects in Solids) returned HTTP 403.'
- 'Bismuth-tin (Bi 58, Sn 42): the tensile strength on American Elements (blocked) was not read, so no mechanical value is recorded for it.'
- 'Bismuth-lead eutectic: the Brinell hardness of 15 is printed without a unit, so it is left out. The 44.1 MPa tensile value and the 37.5% elongation have no test method on the page.'
- 'Bismuth-lead eutectic: the eutectic melting point is 124 °C in the Goodfellow page and the OECD-NEA review, 125 °C in the Wikipedia table, and 123.5 °C in one OECD-NEA passage. All are recorded as printed.'
- 'Rose''s metal composition: the Wikipedia table prints 50/25/25 and the article text gives 25 to 28% lead and 22 to 25% tin. Both are recorded as printed.'
- No corrosion, oxidation or galvanic-corrosion data were found for the solid alloys. The only corrosion statement is the qualitative OECD-NEA remark on molten LBE.
- No UNS, EN, ASTM or JIS designation was found for Rose's, Newton's or Field's metal in any source read.
- No space, vacuum, outgassing, radiation or thermal-cycling data were found. The uses listed are ground uses.
- Field's metal is a bismuth-indium-tin alloy, not bismuth-lead. The brief's bismuth-lead and bismuth-tin scope does not include it, so its data are kept separate in the summary.
sources:
wikipedia-fusible-alloy:
title: Fusible alloy, Wikipedia (well-known alloys table and other alloys table)
url: https://en.wikipedia.org/wiki/Fusible_alloy
kind: web
license: CC BY-SA 4.0, linked not reproduced
wikipedia-roses-metal:
title: Rose's metal, Wikipedia (lead section, uses, history)
url: https://en.wikipedia.org/wiki/Rose%27s_metal
kind: web
license: CC BY-SA 4.0, linked not reproduced
wikipedia-fields-metal:
title: Field's metal, Wikipedia (lead paragraph, toxicity, applications)
url: https://en.wikipedia.org/wiki/Field%27s_metal
kind: web
license: CC BY-SA 4.0, linked not reproduced
wikipedia-newtons-metal:
title: Newton's metal, Wikipedia (lead section)
url: https://en.wikipedia.org/wiki/Newton%27s_metal
kind: web
license: CC BY-SA 4.0, linked not reproduced
wikipedia-bismuth:
title: Bismuth, Wikipedia (physical properties and toxicity)
url: https://en.wikipedia.org/wiki/Bismuth
kind: web
license: CC BY-SA 4.0, linked not reproduced
wikipedia-lead:
title: Lead, Wikipedia (toxicity)
url: https://en.wikipedia.org/wiki/Lead
kind: web
license: CC BY-SA 4.0, linked not reproduced
wikipedia-indium:
title: Indium, Wikipedia (occurrence and toxicity)
url: https://en.wikipedia.org/wiki/Indium
kind: web
license: CC BY-SA 4.0, linked not reproduced
goodfellow-bipb:
title: Bismuth-lead alloy pellets, 55.5:44.5 eutectic (Goodfellow Metals)
url: https://www.goodfellow.com/usa/bismuth-lead-alloy-pellets-bi55-5-pb44-5-group
kind: datasheet
license: supplier page, cited not reproduced
goodfellow-bisn:
title: Bismuth/tin alloy ingot, Bi58/Sn42 (Goodfellow Metals)
url: https://www.goodfellow.com:443/p/bi11-lp-000100/bismuth-tin-alloy-ingot
kind: datasheet
license: supplier page, cited not reproduced
aim-alloy-information:
title: Alloy information, common and specialty solder alloys (AIM Solder)
url: https://aimsolder.com/wp-content/uploads/legacy-files/alloy_information.pdf
kind: datasheet
license: supplier document, cited not reproduced
oecd-nea-lbe:
title: 'Lead-bismuth eutectic: thermophysical and electric properties, chapter 2 (OECD Nuclear Energy Agency, 2007)'
url: https://www.oecd-nea.org/science/reports/2007/pdf/chapter2.pdf
kind: report
license: OECD-NEA, cited not reproduced
usgs-mcs2026-bismuth:
title: 'Mineral Commodity Summaries 2026: Bismuth (U.S. Geological Survey)'
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-bismuth.pdf
kind: report
license: public domain (USGS)
usgs-mcs2026-lead:
title: 'Mineral Commodity Summaries 2026: Lead (U.S. Geological Survey)'
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-lead.pdf
kind: report
license: public domain (USGS)
usgs-mcs2026-tin:
title: 'Mineral Commodity Summaries 2026: Tin (U.S. Geological Survey)'
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-tin.pdf
kind: report
license: public domain (USGS)
usgs-mcs2026-indium:
title: 'Mineral Commodity Summaries 2026: Indium (U.S. Geological Survey)'
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-indium.pdf
kind: report
license: public domain (USGS)
usgs-crit2025:
title: About the 2025 List of Critical Minerals (U.S. Geological Survey)
url: https://www.usgs.gov/programs/mineral-resources-program/science/about-2025-list-critical-minerals
kind: report
license: public domain (USGS)
pubchem-lead:
title: 'PubChem compound record: Lead (CID 5352425), GHS classification'
id: CID 5352425
url: https://pubchem.ncbi.nlm.nih.gov/compound/5352425
kind: database
license: public domain (NCBI)
pubchem-indium:
title: 'PubChem compound record: Indium (CID 5359967), GHS classification'
id: CID 5359967
url: https://pubchem.ncbi.nlm.nih.gov/compound/Indium
kind: database
license: public domain (NCBI)
pubchem-bismuth:
title: 'PubChem compound record: Bismuth (CID 5359367), GHS classification'
id: CID 5359367
url: https://pubchem.ncbi.nlm.nih.gov/compound/Bismuth
kind: database
license: public domain (NCBI)
license: CC-BY-4.0
updated: '2026-10-26'
review:
status: draft
method: assistant
checked_values: 14
unreachable: 4
caveats: 5
note: 'Read by an AI assistant on 2026-10-26. Fourteen numeric properties are sourced: four melting points (Rose''s metal 98 and 94 to 98, Newton''s 97, Field''s 62), two bismuth-lead eutectic melting points (124 from a supplier and the OECD-NEA review), bismuth-lead density, tensile, elongation, resistivity, specific heat and conductivity (supplier), and bismuth-tin melting point (AIM) and density (supplier). Unreachable: Thermo Fisher, Sigma-Aldrich, American Elements (blocked) and the 2007 Newton''s metal paper (HTTP 403). Caveats: the Bi-Pb values come from one supplier and carry no test method; the Wikipedia values have no test conditions; Field''s metal is not bismuth-lead; no corrosion data for solid alloys; the Rose''s metal density is missing.'
story:
recipe:
line: Rose's metal is a bismuth-lead-tin alloy, not a eutectic, with nominal composition 50% bismuth, 25% lead and 25% tin by mass (Wikipedia table). The article gives a wider range of 25 to 28% lead and 22 to 25% tin. The sources read do not describe how the alloy is made.
parts:
- name: Bismuth
symbol: Bi
share_percent: 50
role: The largest share. It makes up half the alloy and gives it a low melting point. Wikipedia describes elemental bismuth as having unusually low toxicity for a heavy metal.
- name: Lead
symbol: Pb
share_percent: 25
role: A heavy, soft component. Its share is 25 to 28% in the article text. Lead is the reason for most of the toxicity warnings in this profile.
- name: Tin
symbol: Sn
share_percent: 25
role: A component that adds to the low melting point. The article gives 22 to 25% tin.
risk_groups:
- title: For people
level: 2
verdict: Lead and indium compounds are toxic
lead: The alloys that contain lead carry lead's hazard codes. Field's metal contains indium, whose compounds are toxic when inhaled, according to Wikipedia.
points:
- label: Lead
line: PubChem's ECHA aggregate for lead reports H360FD, H362, H400 and H410, with signal word Danger. Wikipedia says lead is poisonous whether inhaled or swallowed.
- label: Indium
line: PubChem's indium record lists H302, H312, H315, H319, H332, H335 and H372 with signal word Danger. Field's metal is about 51% indium.
- label: Bismuth
line: Wikipedia says elemental bismuth has unusually low toxicity for a heavy metal. PubChem's bismuth record has no GHS classification, with 324 of 382 company reports not meeting GHS criteria.
- title: If it overheats
lead: These alloys melt well below 150 °C, so a part in service can lose its shape or release its load above the melting point.
points:
- label: Rose's metal
line: The alloy melts between 94 and 98 °C (article), and the Wikipedia table gives 98 °C for the 50/25/25 composition.
- label: Newton's metal
line: Newton's metal melts at 97 °C.
- label: Field's metal
line: Field's metal becomes liquid at about 62 °C (144 °F).
- title: Handling and storage
points:
- label: Lead-bearing alloys
line: PubChem's lead record lists precautionary codes P260, P264, P270 and P280. Wikipedia says lead is toxic whether inhaled or swallowed. Dust and fume control is advice, not a figure from the sources.
- label: Solder mixing
line: Wikipedia warns that combining the bismuth-tin eutectic with lead-tin solder may dramatically lower the melting point and lead to joint failure.
why: 'Rose''s metal is a low-melting alloy of bismuth, lead and tin, and Newton''s metal is a close relative. Their melting points are low enough for heat-transfer baths and fusible releases. Field''s metal trades a lead-free composition for a lower melting point (about 62 °C) and a high cost, since indium is expensive. The bismuth-lead eutectic is the coolant alloy in the OECD-NEA review, and the bismuth-tin eutectic is listed in the AIM solder table. Wikipedia gives the history of Rose''s metal: the German chemist Valentin Rose the Elder discovered it.'
uses:
- where: Heat-transfer baths
line: Wikipedia says Rose's metal is used as a heat-transfer medium in heating baths. It is also used as a solder, to set cast iron railings in stone, and as a filler that keeps tubes from crimping while they are bent.
- where: Radiation treatment shielding
line: Wikipedia says Newton's metal is comparable to Cerrobend without Cerrobend's cadmium, which has encouraged its use for easily shaped shielding in radiotherapy. This is a ground medical use.
- where: Low-temperature solder
line: The AIM Solder alloy sheet lists the bismuth-tin eutectic, Bi58 with 138 °C melting point, among its specialty solder alloys. Wikipedia notes the alloy has reasonable shear strength and fatigue properties.
can_do:
- label: Melt low
value: 98 °C melting point
benchmark: melting_point
line: Rose's metal melts at 98 °C in the Wikipedia table and between 94 and 98 °C in its article. Newton's metal melts at 97 °C.
- label: Melt lower
value: 62 °C melting point
benchmark: melting_point
line: Field's metal, the bismuth-indium-tin eutectic, becomes liquid at about 62 °C (144 °F).
- label: Weight
value: 10.44 g/cm3 density
benchmark: density
line: The bismuth-lead eutectic has a density of 10.44 g/cm3 on a supplier page. The bismuth-tin eutectic is 8.56 g/cm3 on another supplier page. No density is recorded for Rose's metal.
- label: Strength
value: 44.1 MPa tensile
benchmark: ultimate_tensile_strength
line: The bismuth-lead eutectic has a tensile strength of 44.1 MPa on a supplier page, without a test method. It stretches 37.5% before it breaks.
compare: These alloys sit at the low-melting end of the metal family. Rose's metal and Newton's metal melt at 97 to 98 °C, 27 to 28 °C above Wood's metal (70 °C in the Wikipedia table), and both carry lead rather than cadmium. Field's metal, at about 62 °C, is the lowest of the group, but it is an indium alloy and costs more. The bismuth-lead eutectic at 124 °C and the bismuth-tin eutectic at 138 °C sit above Rose's metal. For the values that exist, the bismuth-lead eutectic is the most complete record.
compare_rows:
- label: Melting point
benchmark: melting_point
- label: Density
benchmark: density
- label: Tensile strength
benchmark: ultimate_tensile_strength
handling:
- Treat lead-bearing alloys as toxic. Wikipedia says lead is poisonous whether inhaled or swallowed. Dust and fume control is advice, not a figure from the sources.
- 'Keep the composition in view: the Rose''s metal melting point in Wikipedia is 98 °C for 50/25/25, while the article gives 94 to 98 °C.'
- Do not mix bismuth-tin solder with lead-tin solder in one joint, since the mixed alloy may fail (Wikipedia).
good_for:
- Heat-transfer baths held near 98 °C, where Rose's metal is used (Wikipedia).
- Fusible releases near 62 °C, where Field's metal is used as a low-melting, lead-free option (Wikipedia).
watch_out:
- 'Lead: Rose''s, Newton''s and the bismuth-lead eutectic contain lead, and PubChem records H360FD and H362 for lead.'
- 'Indium cost: Field''s metal is costly, since its major component is indium, which Wikipedia says costs about double the price of silver.'
- 'Few physical data: no density for Rose''s metal, and no thermal or tensile data for Rose''s, Newton''s or Field''s metal in any source read.'
verdict: Rose's metal and Newton's metal are lead-containing fusible alloys that melt at 97 to 98 °C. Field's metal is a lead-free, indium-based alternative at 62 °C. The bismuth-lead and bismuth-tin eutectics have the most complete data. The physical data for the three named alloys are thin, and lead's toxicity is the main hazard.
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.