Nickel oxide NiO
NiO · CAS 1313-99-1 · cubic, Fm3m
Nickel(II) oxide (NiO) is a green-to-black oxide with a face-centred cubic rock-salt structure.
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
p-type conduction
7.2 S/cm at 110 nm
Higher conductivity film
9.09 S/cm at 100 nm
Crystal cell
4.169 Å cubic lattice
Scale stress
about 10 MN/m2 at 1000 °C
Recipe, share of the weight
- Ni not statedNickel
- O not statedOxygen
Best for
p-type transparent conducting films and nickel-based solid oxide fuel cell anode work, under strict dust and inhalation controls
Weakest at
Low conductivity in sputtered films (7.2 to 9.09 S/cm) and a carcinogen hazard (H350, with IARC Group 1 for nickel compounds)
Risk at a glance
- People Low. Cancer risk by inhalation; skin sensitiser
- If it fails Moderate. Growth stress in a NiO scale on nickel at high temperature
- Corrosion Moderate. The NiO scale grows outward and pushes sideways with a stress of about 10 MN/m2, so it is not a passive layer.
Quick facts: NiO
| Property | Value | Basis |
|---|---|---|
| Density | 6.67 g/cm³ | 2 sourced values across conditions |
| Melting point | 1,984 °C | 1 sourced value |
What is the density of Nickel oxide (NiO)?
Nickel oxide (NiO) has a density of 6.67 g/cm³. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the melting point of Nickel oxide (NiO)?
Nickel oxide (NiO) has a melting point of 1,984 °C. The source and test conditions are listed in the properties table on this page.
What is Nickel oxide (NiO) used for?
Uses recorded in the sources include p-type transparent conducting layer in transparent p-n junctions and thin-film transistors; Solid oxide fuel cell anode made from porous Ni/YSZ or NiO/YSZ composites; Oxide scale on nickel and nickel-base alloys in hot oxidising gas.
Why it exists
Nickel oxide is a simple rock-salt oxide and the p-type counterpart to n-type transparent oxides such as zinc oxide. Its record in the sources read is in three places: sputtered films that conduct as p-type layers (7.2 and 9.09 S/cm, with 40 to 69 percent transmittance), porous Ni/YSZ and NiO/YSZ composites studied as solid oxide fuel cell anodes, and a NiO scale on nickel that builds a compressive stress of about 10 MN/m2 at 1000 °C. Its weak point is the hazard: the SDS classes it as a carcinogen and IARC places nickel compounds in Group 1. No flight or space-exposure data for NiO was found.
Where it's used
Transparent p-type layers
The 2024 review calls NiO the first p-type transparent conducting oxide. It is mostly used in transparent p-n junctions and thin-film transistors.
Solid oxide fuel cell anodes
A 2006 Waterloo thesis studied porous Ni/YSZ and NiO/YSZ composites with nickel loadings from 4 to 77 vol%, and found the nickel loading must stay in a window to keep conductivity and avoid thermal mismatch with the electrolyte.
Oxide scale on nickel and nickel alloys
A NiO scale on nickel at 1000 °C in oxygen carries a compressive stress of about 10 MN/m2. The NASA report expects its results to apply to nickel-base alloys.
Recipe
NiO
NiO is a 1:1 compound of nickel and oxygen. It crystallises in the face-centred cubic rock-salt structure (space group Fm3m), with a lattice constant of 4.169 Å at 298 K. Simple rock-salt structure is one reason the 2024 review gives for its use as a p-type transparent conductor.
| Ingredient | Share of the weight | What it does |
|---|---|---|
| Nickel Ni | not stated | The metal cation. Ni(II) ions sit in the rock-salt lattice with oxygen as the counter-ion. |
| Oxygen O | not stated | The anion. Oxygen forms the other half of the rock-salt lattice with nickel. |
Weight shares are as printed in the sources.
What it can do
p-type conduction
7.2 S/cm at 110 nm
A 110 nm sputtered NiO film on glass conducts at 7.2 S/cm with 40 percent average transmittance.
Higher conductivity film
9.09 S/cm at 100 nm
An RF-sputtered 100 nm NiO film reached 9.09 S/cm, 69 percent transmittance and 6.12 cm2/V-s Hall mobility.
Crystal cell
4.169 Å cubic lattice
The rock-salt cell has a lattice constant of 4.169 Å at 298 K from X-ray refinement.
Scale stress
about 10 MN/m2 at 1000 °C
Nickel oxide grown on nickel in oxygen at 1000 °C carries a grain-boundary pressure of about 10 MN/m2.
How it compares
Compared with zinc oxide, nickel oxide melts at a higher temperature and is denser, as the compare rows show. Its sputtered-film conductivity (7.2 to 9.09 S/cm) is for an undoped p-type film, so it is not directly comparable with the doped n-type zinc oxide films. The main difference is the hazard: zinc oxide is classed only as an aquatic hazard in its SDS, while nickel oxide carries a carcinogen classification.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | NiO | Al2O3 | BaTiO3 | BeO | CaTiO3 | RCF | CeO2 | CoO and Co3O4 | CuO, Cu2O | HfO2 | Fe2O3, Fe3O4 | LSM | PZT | MgO | Nb2O5 | Al2Si4O10(OH)2 | Ln2O3 | SiO | MgO-SiO2 | SnO2, ITO | TiO2 | WO3 | V2O5 | Y2O3 | ZnO | Mg-PSZ, ATZ, ZTA | YSZ |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Thermal behavior and safety | |||||||||||||||||||||||||||
| Melting point, nickel oxide (Angstrom Sciences SDS)Value printed in a supplier safety data sheet | 1984 °C2 | 2030 to 2072 °C | 1625 °C | 2578 °C | 1975 °C | 1760 °C | 2600 °C | 1830 °C | 1326 °C | 2774 °C | no data | no data | no data | 2800 °C | 1500 °C | no data | 2304 °C | 1702 °C | no data | 1630 °C | 1850 °C | 1472 °C | 690 °C | 2410 °C | 1975 °C | no data | no data |
| Physical and electrical | |||||||||||||||||||||||||||
| Relative density, nickel(II) oxide (Sigma-Aldrich SDS) | 6.67 g/cm³1 | 3.72 g/cm³ | 6.08 - | 3.01 g/cu cm | 4.1 g/cc | 64 kg/m3 | 7.65 g/cm³ | 6.45 g/cm³ | 6 - | 9.68 g/cc | 5.24 g/cm³ | 2 g/cm³ | 7.8 g/cm³ | 3.58 g/cm³ | 4.6 g/cm³ | 2.3 g/cc | 6.51 g/cm³ | 2.13 g/cc | 2.8 g/cm³ | 6.95 g/mL | 4 g/cm³ | 7.2 g/cm³ | 3.4 - | > 4.9 g/cm³ | 5.67 g/cm³ | 5.72 g/cm³ | 6.02 g/cm³ |
| Density, nickel oxide (Angstrom Sciences SDS)Value printed in a supplier safety data sheet | 6.67 g/cm³ | 3.72 g/cm³ | 6.08 - | 3.01 g/cu cm | 4.1 g/cc | 64 kg/m3 | 7.65 g/cm³ | 6.45 g/cm³ | 6 - | 9.68 g/cc | 5.24 g/cm³ | 2 g/cm³ | 7.8 g/cm³ | 3.58 g/cm³ | 4.6 g/cm³ | 2.3 g/cc | 6.51 g/cm³ | 2.13 g/cc | 2.8 g/cm³ | 6.95 g/mL | 4 g/cm³ | 7.2 g/cm³ | 3.4 - | > 4.9 g/cm³ | 5.67 g/cm³ | 5.72 g/cm³ | 6.02 g/cm³ |
| Electrical conductivity, 110 nm sputtered NiO filmValue tabulated in a 2024 review (Table 4) | 7.2 S/cm7 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Electrical conductivity, 100 nm RF-sputtered NiO filmValue tabulated in a 2024 review (Table 4) | 9.09 S/cm9 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Other measurements | |||||||||||||||||||||||||||
| Molecular weight, nickel oxide (computed) | 74.69 g/mol3 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | 231.8 g/mol | no data | no data | no data | no data | no data |
| Water solubility, nickel oxide at 20 °C | 3×10^-5 g/l4 | no data | no data | 2 ug/100 mL | no data | no data | no data | 4.88 mg/L | no data | no data | no data | no data | no data | 86 mg/L | no data | no data | no data | no data | no data | no data | no data | no data | 0.8 g/100ml | no data | no data | no data | no data |
| Optical band gap, single-crystal NiO (range) | 3.6 to 4 eV5 | no data | no data | 10.6 eV | no data | no data | no data | no data | 2.17 eV | 5.65 eV | no data | no data | no data | no data | no data | no data | no data | no data | no data | 3.6 eV | 3.23 eV | no data | no data | no data | 3.37 eV | no data | no data |
| Optical band gap, 110 nm sputtered NiO film on glass | 3.8 eV6 | no data | no data | 10.6 eV | no data | no data | no data | no data | 2.17 eV | 5.65 eV | no data | no data | no data | no data | no data | no data | no data | no data | no data | 3.6 eV | 3.23 eV | no data | no data | no data | 3.37 eV | no data | no data |
| Average transmittance, 110 nm sputtered NiO filmValue tabulated in a 2024 review (Table 4) | 40 %8 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | 79.4 % | no data | no data | no data | no data | 80.88 % | no data | no data | no data | no data | > 85 % | no data | no data |
| Average transmittance, 100 nm RF-sputtered NiO filmValue tabulated in a 2024 review (Table 4) | 69 %10 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | 79.4 % | no data | no data | no data | no data | 80.88 % | no data | no data | no data | no data | > 85 % | no data | no data |
| Hall mobility, 100 nm RF-sputtered NiO filmValue tabulated in a 2024 review (Table 4) | 6.12 cm²/V-s11 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Lattice constant a, NiO single crystal at 298 K | 4.169 Å12 | no data | no data | 2.698 Å | no data | no data | no data | no data | 4.23 Å | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | 0.3785 nm | no data | no data | no data | 3.25 Å | no data | no data |
Why choose it, and why not
Good for
- Undoped p-type transparent layers in research devices, at 7.2 to 9.09 S/cm in sputtered films.
- Nickel-based solid oxide fuel cell anode work, where the NiO/YSZ composite is the starting material.
- Studying oxide scale growth on nickel at high temperature, where the scale stress is about 10 MN/m2 at 1000 °C.
Watch out for
- The carcinogen classification: H350 in the Sigma-Aldrich SDS, H350i in the paste SDS, and IARC Group 1 for nickel compounds.
- Volume change of nickel on oxidation in anodes, and the scale growth stress on nickel.
- Hazard classes differ between the SDS sheets read, and the PubChem summary is mixed.
Nickel oxide is a simple, well-characterised p-type oxide, with film conductivity of about 7 to 9 S/cm in the sources read. Its carcinogen classification and dust hazard make it a controlled material. It has no flight record, and the battery-precursor use is not backed by a source read in this run, so it is listed as a gap.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Relative density, nickel(II) oxide (Sigma-Aldrich SDS) | Value printed in a supplier safety data sheet as relative density | temperature 25 °C (77 °F)grade powder, Sigma-Aldrich product 637130 | — |
| 2 | Melting point, nickel oxide (Angstrom Sciences SDS) | — | grade powder, as listed in the SDS | The Sigma-Aldrich SDS for the same compound gives melting point as No data available, so this value rests on one reseller sheet. |
| 3 | Molecular weight, nickel oxide (computed) | Computed molecular weight printed in the PubChem record | basis computed property in the database record | — |
| 4 | Water solubility, nickel oxide at 20 °C | OECD Test Guideline 105, as printed in the supplier safety data sheet | temperature 20 °C (68 °F) | The SDS describes the product as practically insoluble. |
| 5 | Optical band gap, single-crystal NiO (range) | Range stated in a 2024 review of p-type transparent conducting oxides | crystal single crystaltemperature not stated in the review | — |
| 6 | Optical band gap, 110 nm sputtered NiO film on glass | Value tabulated in a 2024 review (Table 4) from the study it cites as reference [5] | film thickness 110 nmsubstrate glassdeposition magnetron sputtering | — |
| 7 | Electrical conductivity, 110 nm sputtered NiO film | — | film thickness 110 nmsubstrate glassdeposition magnetron sputtering | — |
| 8 | Average transmittance, 110 nm sputtered NiO film | — | film thickness 110 nmsubstrate glassdeposition magnetron sputtering | — |
| 9 | Electrical conductivity, 100 nm RF-sputtered NiO film | — | film thickness 100 nmsubstrate glassdeposition RF magnetron sputtering | — |
| 10 | Average transmittance, 100 nm RF-sputtered NiO film | — | film thickness 100 nmsubstrate glassdeposition RF magnetron sputtering | — |
| 11 | Hall mobility, 100 nm RF-sputtered NiO film | — | film thickness 100 nmsubstrate glassdeposition RF magnetron sputtering | — |
| 12 | Lattice constant a, NiO single crystal at 298 K | Least-squares refinement of X-ray diffraction data, printed as 4.169(2) Å | crystal single crystal, face-centred cubic (Fm3m)temperature 298 K | The paper prints the uncertainty as (2) in the last digit. |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Nickel heated in dry oxygen at 1000 °C (NiO scale on nickel) | moderate | The NiO scale grows outward and pushes sideways with a stress of about 10 MN/m2, so it is not a passive layer.1 |
| Ni/NiO-YSZ composites in a solid oxide fuel cell anode, through burnout and redox cycling | moderate | Nickel expands when it oxidises, so the anode composition has to stay within a window that also avoids thermal mismatch with the electrolyte.2 |
| Water (practically insoluble) | not rated | The supplier SDS shows negligible dissolution in water, but gives no corrosion rate.3 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Nickel heated in dry oxygen at 1000 °C (NiO scale on nickel) | The NASA report says nickel oxide growing on nickel in oxygen at 1000 °C has a mean grain-boundary pressure of approximately 10 MN/m2, and that the scale is not passive because it generates a lateral compressive stress during oxidation. The scale thickens almost exclusively by outward diffusion of metal ions through the oxide. | temperature 1000 °Catmosphere oxygensubstrate nickel (Nickel-201 and Nickel-270 in the report) |
| 2 | Ni/NiO-YSZ composites in a solid oxide fuel cell anode, through burnout and redox cycling | The Waterloo thesis abstract says the composites made from nickel metal expand due to nickel oxidation during burnout, while the composites that started from NiO change little in volume on reduction when YSZ is present. It limits nickel loading to a window with a minimum for electrical conductivity and a maximum to avoid thermal mismatch with YSZ. | nickel loading 4 to 77 vol% of total solids (range studied)process burnout and reduction of porous composites |
| 3 | Water (practically insoluble) | The Sigma-Aldrich SDS gives a water solubility of 0.00003 g/l at 20 °C and describes the product as practically insoluble. The SDS gives no corrosion rate, so the rating is unknown. | temperature 20 °C |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
The supplier safety data sheets classify nickel oxide as a Danger-level carcinogen and skin sensitiser. IARC places nickel compounds in Group 1.
- Inhalation
- The Sigma-Aldrich SDS gives H350 (may cause cancer) and H372 (organ damage from repeated exposure). The paste SDS gives H350i (cancer by inhalation).
- Dust limits
- OSHA PEL 1 mg/m3, NIOSH REL 0.015 mg/m3 (potential carcinogen), and ACGIH TLV 0.2 mg/m3 are the workplace limits printed in the SDS.
- Skin
- H317 means it can cause an allergic skin reaction.
If the oxide is heated or cycled
High-temperature oxidation and redox cycling change the stress and the volume of nickel-based parts.
- Scale stress
- On nickel at 1000 °C in oxygen, the NiO scale carries a compressive stress of about 10 MN/m2.
- Anode cycling
- In Ni/YSZ composites, nickel expands when it oxidises, so the nickel loading has to stay in a window.
Handling and storage
- Dust
- Avoid dust formation and provide exhaust ventilation. Clean up spills without creating dust.
- Storage
- Handle and store under inert gas, in a dry place, as the Sigma-Aldrich SDS says.
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Growth stress in a NiO scale on nickel at high temperaturemoderate severity | Heating nickel in oxygen at about 1000 °C for long periodsThe scale carries a compressive grain-boundary stress of about 10 MN/m2, which the NASA report models as a change to the high-temperature creep behaviour of the nickel beneath it. |
| Volume change of nickel in a fuel cell anode on redox cyclingmoderate severity | Oxidation of the nickel phase during burnout or a loss of reducing gas in serviceExpansion of the nickel phase can break the match with the YSZ electrolyte, so the nickel loading has to stay inside a narrow window. |
Handling and storage
- Avoid contact with skin and eyes and avoid forming dust. Provide exhaust ventilation where dust is formed. Combustible dust can form in further processing.
- Handle and store under inert gas, in a dry place.
- Pick up spills without creating dust, sweep up or shovel, and keep the waste in closed containers.
Mitigations
- Workplace limits in the SDS: OSHA PEL 1 mg/m3 TWA, NIOSH REL 0.015 mg/m3 TWA (potential occupational carcinogen), ACGIH TLV 0.2 mg/m3 TWA (confirmed human carcinogen, lung cancer).
- NIOSH lists the IDLH for nickel metal and other compounds as 10 mg/m3 as Ni. The NIOSH entry does not state the basis for this value on the page read.
- Where a risk assessment shows that respirators are needed, the SDS recommends a full-face particle respirator (N100 or P3 cartridges) as a backup to engineering controls.
Supply and geography
How common the raw materials are and where they come from.
Nickel (feedstock for NiO)
- Top producers (2025)
- Indonesia 66.7%, Philippines 6.9%, Russia 5.1%, New Caledonia 3.6%, Canada 3.6%, China 3.1%, Brazil 1.8%, Australia 1.2%, United States 0.3%
- Critical mineral lists
- US: listed
- Recycling
- USGS: nickel recovered from scrap was about 60 percent of US apparent consumption in 2025, mostly from stainless-steel scrap.
- Substitutes
- USGS nickel chapter: low-nickel, duplex or ultrahigh-chromium stainless steels can replace austenitic grades, and titanium alloys can replace nickel-base alloys in corrosive environments.
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: nickel-oxide
spore_version: 0.2
family: oxide-ceramics
name: Nickel oxide
abbreviation: NiO
role: p-type oxide for transparent layers, solid oxide fuel cell anodes and oxide scales on nickel; carcinogen
category: ceramics
type: oxides
summary: |
Nickel(II) oxide (NiO) is a green-to-black oxide with a face-centred cubic rock-salt structure. Its lattice constant is 4.169 Å at 298 K, its density is 6.67 g/cm3, and one supplier safety data sheet gives a melting point of 1984 °C. It is practically insoluble in water (0.00003 g/l at 20 °C). Sputtered NiO films are p-type conductors: a 110 nm film on glass reached 7.2 S/cm with 40 percent average transmittance, and a 100 nm RF-sputtered film reached 9.09 S/cm with 69 percent. Porous Ni/YSZ and NiO/YSZ composites have been studied for solid oxide fuel cell anodes. Nickel heated in oxygen forms a NiO scale that grows outward and carries a compressive grain-boundary stress of about 10 MN/m2 at 1000 °C. NiO is a carcinogen hazard: the Sigma-Aldrich safety data sheet gives H350, and IARC places nickel compounds in Group 1.
best_for: p-type transparent conducting films and nickel-based solid oxide fuel cell anode work, under strict dust and inhalation controls
weakest_at: Low conductivity in sputtered films (7.2 to 9.09 S/cm) and a carcinogen hazard (H350, with IARC Group 1 for nickel compounds)
identity:
formula: NiO
cas: 1313-99-1
crystal_system: cubic
space_group: Fm3m
source: vidal-2005-nio
where: Experimental Procedures, paragraph beginning 'No antiferromagnetic distortion' (face-centred cubic, Fm3m, lattice constant 4.169(2) Å at 298 K); CAS number in Section 3 of sigma-sds-nio
tags:
environments: []
stresses:
- extreme-heat
applications:
- electronics-and-chips
- batteries
- propulsion-and-tanks
properties:
- benchmark: density
label: Relative density, nickel(II) oxide (Sigma-Aldrich SDS)
value: 6.67
unit: g/cm3
scope: material
conditions:
temperature: 25 °C (77 °F)
grade: powder, Sigma-Aldrich product 637130
method: Value printed in a supplier safety data sheet as relative density
status: ground
source: sigma-sds-nio
where: Section 9 (Physical and Chemical Properties), item m) Relative density
- benchmark: density
label: Density, nickel oxide (Angstrom Sciences SDS)
value: 6.67
unit: g/cm3
scope: material
conditions:
grade: powder, sputtering target and custom parts, as listed in the SDS
method: Value printed in a supplier safety data sheet
status: ground
source: angstrom-sds-nio
where: Section 9 (Physical and Chemical Properties), Density row (printed as 6.67 g/cc)
- benchmark: melting_point
label: Melting point, nickel oxide (Angstrom Sciences SDS)
value: 1984
unit: °C
scope: material
conditions:
grade: powder, as listed in the SDS
method: Value printed in a supplier safety data sheet
status: ground
note: The Sigma-Aldrich SDS for the same compound gives melting point as No data available, so this value rests on one reseller sheet.
source: angstrom-sds-nio
where: Section 9 (Physical and Chemical Properties), Melting Point row
- benchmark: molar_mass
label: Molecular weight, nickel oxide (computed)
value: 74.693
unit: g/mol
scope: material
conditions:
basis: computed property in the database record
method: Computed molecular weight printed in the PubChem record
status: calculated
source: pubchem-nio
where: Chemical and Physical Properties, Computed Properties, Molecular Weight
- benchmark: water_solubility
label: Water solubility, nickel oxide at 20 °C
value: 0.00003
unit: g/l
scope: material
conditions:
temperature: 20 °C (68 °F)
method: OECD Test Guideline 105, as printed in the supplier safety data sheet
status: ground
note: The SDS describes the product as practically insoluble.
source: sigma-sds-nio
where: Section 9, item n) Water solubility
- benchmark: band_gap
label: Optical band gap, single-crystal NiO (range)
value: 3.6
value_high: 4
bound: range
unit: eV
scope: material
conditions:
crystal: single crystal
temperature: not stated in the review
method: Range stated in a 2024 review of p-type transparent conducting oxides
status: ground
source: arxiv-ptco-2024
where: Section on NiO, sentence beginning 'However, the optical band energy of single-crystal NiO', citing reference [5] of the review
- benchmark: band_gap
label: Optical band gap, 110 nm sputtered NiO film on glass
value: 3.8
unit: eV
scope: material
conditions:
film_thickness: 110 nm
substrate: glass
deposition: magnetron sputtering
method: Value tabulated in a 2024 review (Table 4) from the study it cites as reference [5]
status: ground
source: arxiv-ptco-2024
where: Table 4 (Binary oxide materials as p-type TCO), NiO row, magnetron sputtering
- benchmark: electrical_conductivity
label: Electrical conductivity, 110 nm sputtered NiO film
value: 7.2
unit: S/cm
scope: material
conditions:
film_thickness: 110 nm
substrate: glass
deposition: magnetron sputtering
method: Value tabulated in a 2024 review (Table 4)
status: ground
source: arxiv-ptco-2024
where: Table 4, NiO row, electrical conductivity column (S/cm)
- benchmark: optical_transmittance
label: Average transmittance, 110 nm sputtered NiO film
value: 40
unit: '%'
scope: material
conditions:
film_thickness: 110 nm
substrate: glass
deposition: magnetron sputtering
method: Value tabulated in a 2024 review (Table 4)
status: ground
source: arxiv-ptco-2024
where: Table 4, NiO row, average transmittance column
- benchmark: electrical_conductivity
label: Electrical conductivity, 100 nm RF-sputtered NiO film
value: 9.09
unit: S/cm
scope: material
conditions:
film_thickness: 100 nm
substrate: glass
deposition: RF magnetron sputtering
method: Value tabulated in a 2024 review (Table 4)
status: ground
source: arxiv-ptco-2024
where: Table 4, NiO RFMS row (reference [96]), electrical conductivity column
- benchmark: optical_transmittance
label: Average transmittance, 100 nm RF-sputtered NiO film
value: 69
unit: '%'
scope: material
conditions:
film_thickness: 100 nm
substrate: glass
deposition: RF magnetron sputtering
method: Value tabulated in a 2024 review (Table 4)
status: ground
source: arxiv-ptco-2024
where: Table 4, NiO RFMS row (reference [96]), average transmittance column
- benchmark: hall_mobility
label: Hall mobility, 100 nm RF-sputtered NiO film
value: 6.12
unit: cm2/V-s
scope: material
conditions:
film_thickness: 100 nm
substrate: glass
deposition: RF magnetron sputtering
method: Value tabulated in a 2024 review (Table 4)
status: ground
source: arxiv-ptco-2024
where: Table 4, NiO RFMS row (reference [96]), Hall mobility column
- benchmark: lattice_constant_a
label: Lattice constant a, NiO single crystal at 298 K
value: 4.169
unit: Å
scope: material
conditions:
crystal: single crystal, face-centred cubic (Fm3m)
temperature: 298 K
method: Least-squares refinement of X-ray diffraction data, printed as 4.169(2) Å
status: ground
note: The paper prints the uncertainty as (2) in the last digit.
source: vidal-2005-nio
where: Experimental Procedures, paragraph after the structure factor table, sentence beginning 'Least-squares refinement'
corrosion:
- environment: Nickel heated in dry oxygen at 1000 °C (NiO scale on nickel)
headline: The NiO scale grows outward and pushes sideways with a stress of about 10 MN/m2, so it is not a passive layer.
effect: The NASA report says nickel oxide growing on nickel in oxygen at 1000 °C has a mean grain-boundary pressure of approximately 10 MN/m2, and that the scale is not passive because it generates a lateral compressive stress during oxidation. The scale thickens almost exclusively by outward diffusion of metal ions through the oxide.
rating: moderate
conditions:
temperature: 1000 °C
atmosphere: oxygen
substrate: nickel (Nickel-201 and Nickel-270 in the report)
source: nasa-tn-d5266
where: 'Section ''Case 2: The active surface layer'' (page 8), and the introduction, point (3)'
- environment: Ni/NiO-YSZ composites in a solid oxide fuel cell anode, through burnout and redox cycling
headline: Nickel expands when it oxidises, so the anode composition has to stay within a window that also avoids thermal mismatch with the electrolyte.
effect: The Waterloo thesis abstract says the composites made from nickel metal expand due to nickel oxidation during burnout, while the composites that started from NiO change little in volume on reduction when YSZ is present. It limits nickel loading to a window with a minimum for electrical conductivity and a maximum to avoid thermal mismatch with YSZ.
rating: moderate
conditions:
nickel_loading: 4 to 77 vol% of total solids (range studied)
process: burnout and reduction of porous composites
source: clemmer-2006-nio-ysz
where: Abstract
- environment: Water (practically insoluble)
headline: The supplier SDS shows negligible dissolution in water, but gives no corrosion rate.
effect: The Sigma-Aldrich SDS gives a water solubility of 0.00003 g/l at 20 °C and describes the product as practically insoluble. The SDS gives no corrosion rate, so the rating is unknown.
rating: unknown
conditions:
temperature: 20 °C
source: sigma-sds-nio
where: Section 9, item n) Water solubility
risks:
hazards:
- text: The Sigma-Aldrich SDS classes nickel(II) oxide as Danger with H317 (allergic skin reaction), H350 (may cause cancer), H372 (organ damage through prolonged or repeated exposure) and H413 (long-lasting harm to aquatic life).
ghs:
- H317
- H350
- H372
- H413
source: sigma-sds-nio
where: Section 2 (Hazards identification), GHS classification
- text: PubChem's summary of ECHA notifications gives the same four codes, with H317 in 100 percent of classifying notifications and H350 in 98.9 percent. The record title reads Nickel trioxide, but the formula NiO and CAS 1313-99-1 match nickel(II) oxide.
ghs:
- H317
- H350
- H372
- H413
source: pubchem-nio
where: Safety and Hazards, GHS Classification, ECHA C&L Notifications Summary
- text: A Solaronix SDS for a nickel oxide paste (Ni-Nanoxide N/SP, nickel monoxide 10 to 25 percent) classes it as Danger with H315, H317, H350i (cancer by inhalation), H372 and H413. It is a paste, so this is a product classification and not a pure NiO classification.
ghs:
- H315
- H317
- H350i
- H372
- H413
source: solaronix-sds-nio
where: Sections 2 and 3 (dangerous components)
- text: IARC classifies nickel compounds in Group 1, carcinogenic to humans, with a definite link to lung, nasal and paranasal cancer. The CAREX Canada profile says the evaluation was mainly for nickel compounds containing oxygen and sulphur. The page does not name nickel oxide directly.
ghs: []
source: carex-nickel
where: Nickel Profile, paragraph on IARC Monograph Vol. 100C (2012)
failure_risks:
- mode: Growth stress in a NiO scale on nickel at high temperature
trigger: Heating nickel in oxygen at about 1000 °C for long periods
consequence: The scale carries a compressive grain-boundary stress of about 10 MN/m2, which the NASA report models as a change to the high-temperature creep behaviour of the nickel beneath it.
severity: moderate
source: nasa-tn-d5266
where: 'Section ''Case 2: The active surface layer'' (page 8)'
- mode: Volume change of nickel in a fuel cell anode on redox cycling
trigger: Oxidation of the nickel phase during burnout or a loss of reducing gas in service
consequence: Expansion of the nickel phase can break the match with the YSZ electrolyte, so the nickel loading has to stay inside a narrow window.
severity: moderate
source: clemmer-2006-nio-ysz
where: Abstract
side_effects: []
handling:
- text: Avoid contact with skin and eyes and avoid forming dust. Provide exhaust ventilation where dust is formed. Combustible dust can form in further processing.
source: sigma-sds-nio
where: Section 7.1 (Precautions for safe handling)
- text: Handle and store under inert gas, in a dry place.
source: sigma-sds-nio
where: Section 7.2 (Conditions for safe storage)
- text: Pick up spills without creating dust, sweep up or shovel, and keep the waste in closed containers.
source: sigma-sds-nio
where: Section 6 (Accidental release measures)
mitigations:
- text: 'Workplace limits in the SDS: OSHA PEL 1 mg/m3 TWA, NIOSH REL 0.015 mg/m3 TWA (potential occupational carcinogen), ACGIH TLV 0.2 mg/m3 TWA (confirmed human carcinogen, lung cancer).'
source: sigma-sds-nio
where: Section 8.1 (Control parameters)
- text: NIOSH lists the IDLH for nickel metal and other compounds as 10 mg/m3 as Ni. The NIOSH entry does not state the basis for this value on the page read.
source: niosh-npg-nickel
where: IDLH heading of the NIOSH Pocket Guide entry
- text: Where a risk assessment shows that respirators are needed, the SDS recommends a full-face particle respirator (N100 or P3 cartridges) as a backup to engineering controls.
source: sigma-sds-nio
where: Section 8.2 (Exposure controls), respiratory protection
uses:
- application: electronics-and-chips
device: p-type transparent conducting layer in transparent p-n junctions and thin-film transistors
example: The 2024 review calls NiO the first p-type transparent conducting oxide. Sputtered NiO films in its Table 4 reach 7.2 S/cm with 40 percent transmittance (110 nm) and 9.09 S/cm with 69 percent transmittance (100 nm, RF sputtering).
source: arxiv-ptco-2024
where: Introduction and NiO discussion; Table 4, NiO rows
- application: batteries
device: Solid oxide fuel cell anode made from porous Ni/YSZ or NiO/YSZ composites
example: A 2006 Waterloo thesis studied porous Ni/YSZ and NiO/YSZ composites for solid oxide fuel cells, with nickel loadings from 4 to 77 vol%. The abstract reports that nickel-metal composites expand on oxidation during burnout.
source: clemmer-2006-nio-ysz
where: Abstract
- application: propulsion-and-tanks
device: Oxide scale on nickel and nickel-base alloys in hot oxidising gas
example: A NASA report on oxidation of nickel at 1000 °C models the growing NiO scale and says the results should carry over to complex nickel-base alloy systems. This is a stated expectation, not a measured alloy result.
source: nasa-tn-d5266
where: Introduction, point (4)
supply:
- subject: Nickel (feedstock for NiO)
producers:
- country: Indonesia
share_percent: 66.7
year: 2025
- country: Philippines
share_percent: 6.9
year: 2025
- country: Russia
share_percent: 5.1
year: 2025
- country: New Caledonia
share_percent: 3.6
year: 2025
- country: Canada
share_percent: 3.6
year: 2025
- country: China
share_percent: 3.1
year: 2025
- country: Brazil
share_percent: 1.8
year: 2025
- country: Australia
share_percent: 1.2
year: 2025
- country: United States
share_percent: 0.3
year: 2025
critical_lists:
- list: USGS 2025 List of Critical Minerals (nickel is on the final list, used to make high-strength steel and rechargeable batteries)
listed: true
recycling: 'USGS: nickel recovered from scrap was about 60 percent of US apparent consumption in 2025, mostly from stainless-steel scrap.'
substitutes:
- 'USGS nickel chapter: low-nickel, duplex or ultrahigh-chromium stainless steels can replace austenitic grades, and titanium alloys can replace nickel-base alloys in corrosive environments.'
source: usgs-mcs2026-nickel
where: World Mine Production and Reserves table, 2025e column (world total 3,900,000 t, rounded); Recycling; Substitutes. The producer shares are calculated by Space Mushroom from each tonnage divided by the 3,900,000 t world total, not printed by USGS. USGS gives no NiO production table.
documents:
- title: Sigma-Aldrich safety data sheet, nickel(II) oxide, product 637130 (Version 4.10, revision 28 February 2015; copy hosted by Utah NanoFab)
type: sds
url: https://www.nanofab.utah.edu/wp-content/uploads/2018/08/NickelII-oxide-Sigma-Aldrich-28Feb15_v4.1.pdf
year: 2015
- title: Angstrom Sciences safety data sheet, Nickel Oxide (CAS 1313-99-1; last revision 07/02/15)
type: sds
url: https://angstromsciences.com/wp-content/uploads/files/SDS/Nickel%20Oxide.pdf
year: 2015
- title: Solaronix safety data sheet, Ni-Nanoxide N/SP (nickel oxide paste, EU CLP format; printed 25.06.2013)
type: sds
url: https://www.solaronix.com/msds/MSDS_Ni-Nanoxide_N__SP.pdf
year: 2013
- title: PubChem compound record, CID 14805 (formula NiO, CAS 1313-99-1)
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/14805
year: 2026
- title: 'Progress in Developing Highly Efficient p-Type TCOs for Transparent Electronics: A Comprehensive Review (arXiv 2405.14354)'
type: paper
url: https://arxiv.org/pdf/2405.14354
year: 2024
- title: 'Indications of the Magnetic State in the Charge Distributions of MnO, CoO, and NiO. III: Antiferromagnetism of NiO (Crystallography Reports, 2005)'
type: paper
url: https://www.mv.helsinki.fi/home/kurkisuo/6.1.A/05-NiO.pdf
year: 2005
- title: A Proposed Model for the Effect of Oxidation on the High-Temperature Deformation of Nickel (NASA TN D-5266)
type: report
url: https://ntrs.nasa.gov/api/citations/19690017683/downloads/19690017683.pdf
year: 1969
- title: The Processing and Characterization of Porous Ni/YSZ and NiO/YSZ Composites used in Solid Oxide Fuel Cell Applications (University of Waterloo, 2006)
type: paper
url: https://uwspace.uwaterloo.ca/handle/10012/2883
year: 2006
- title: CAREX Canada, Nickel profile (IARC Monograph Vol. 100C classification)
type: report
url: https://www.carexcanada.ca/?p=9614
year: 2026
- title: 'USGS Mineral Commodity Summaries 2026: Nickel'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-nickel.pdf
year: 2026
- title: NIOSH Pocket Guide, Nickel metal and other compounds (as Ni)
type: report
url: https://www.cdc.gov/niosh/npg/npgd0445.html
year: 2026
gaps:
- No battery-precursor source for NiO was read. The open-access 2022 review (Entwistle et al., Energy Reports) and the 2025 review describe hydroxide precursors milled with a lithium salt. A patent snippet says NiO forms as an intermediate when Ni(OH)2 is heated at 500 °C, but the patent was not fetched, so the battery-precursor use is not stated as a source-backed use.
- The protective Cr2O3 scale and the spallation behaviour of NiO on Ni-Cr and Ni-Mo-Cr alloys were seen only in search snippets. No open alloy-oxidation source was opened, so the alloy claim is limited to the NASA statement that its results should apply to nickel-base alloys.
- Bulk thermal expansion coefficient, thermal conductivity and the Néel temperature were not read in a fetched source in this run. The Néel temperature of 523 K appeared only in a search snippet.
- Molar volume and the NiO/Ni volume change on reduction were in a 2011 MDPI review that returned HTTP 403, so they are not used.
- The IARC Volume 100C monograph was not opened. The Group 1 statement rests on the CAREX Canada profile. The CAREX page does not name nickel oxide directly.
- Atomic weights for nickel and oxygen were not read in a source opened for this profile, so the recipe parts carry no atomic_weight.
- Acid and base attack rates were not found in a source read in this run.
- The PubChem record CID 14805 has the title Nickel trioxide while the formula and CAS number match nickel(II) oxide; PubChem's own melting point and density were not used because the experimental-properties page returned a verification screen.
- Electrical conductivity, band gap, water solubility, molar mass, Hall mobility and lattice constant are not in property-canon.yaml; snake_case names were used, as in zinc-oxide.yaml.
- The H350 (Sigma-Aldrich, PubChem) and H350i (Solaronix paste) classifications differ; both are kept with their source.
- The melting point of 1984 °C comes from one reseller SDS; the Sigma-Aldrich SDS gives no melting point.
- The NASA Tech Brief on black nickel plating (1974) describes a nickel plating process, not NiO, and was not used.
- No flight, vacuum or space-exposure result for NiO was found in the sources read.
- The EU critical raw materials list was not checked for nickel. Crustal abundance of nickel was not read.
sources:
pubchem-nio:
title: PubChem compound record, CID 14805 (formula NiO, CAS 1313-99-1; record title reads Nickel trioxide)
id: CID 14805
url: https://pubchem.ncbi.nlm.nih.gov/rest/pug_view/data/compound/14805/JSON
year: 2026
kind: database
license: public domain (NCBI)
sigma-sds-nio:
title: Sigma-Aldrich safety data sheet, nickel(II) oxide, product 637130 (Version 4.10, revision 28 February 2015)
id: CAS 1313-99-1, product 637130
url: https://www.nanofab.utah.edu/wp-content/uploads/2018/08/NickelII-oxide-Sigma-Aldrich-28Feb15_v4.1.pdf
year: 2015
kind: datasheet
license: supplier document, linked not reproduced
angstrom-sds-nio:
title: Angstrom Sciences safety data sheet, Nickel Oxide (last revision 07/02/15)
id: CAS 1313-99-1, EC 215-215-7
url: https://angstromsciences.com/wp-content/uploads/files/SDS/Nickel%20Oxide.pdf
year: 2015
kind: datasheet
license: supplier document, linked not reproduced
solaronix-sds-nio:
title: Solaronix safety data sheet, Ni-Nanoxide N/SP (nickel oxide paste)
id: printed 25.06.2013, version 1
url: https://www.solaronix.com/msds/MSDS_Ni-Nanoxide_N__SP.pdf
year: 2013
kind: datasheet
license: supplier document, linked not reproduced
arxiv-ptco-2024:
title: 'Progress in Developing Highly Efficient p-Type TCOs for Transparent Electronics: A Comprehensive Review (Singh and Bhardwaj)'
id: arXiv 2405.14354
url: https://arxiv.org/pdf/2405.14354
year: 2024
kind: paper
license: arXiv preprint (cited, not reproduced)
vidal-2005-nio:
title: 'Indications of the Magnetic State in the Charge Distributions of MnO, CoO, and NiO. III: Antiferromagnetism of NiO (Vidal, Vidal-Valat and Kurki-Suonio; Crystallography Reports, vol. 50, no. 1, 2005)'
id: Crystallography Reports 50(1), pp. 20 to 26
url: https://www.mv.helsinki.fi/home/kurkisuo/6.1.A/05-NiO.pdf
year: 2005
kind: paper
license: not stated on the copy read
nasa-tn-d5266:
title: A Proposed Model for the Effect of Oxidation on the High-Temperature Deformation of Nickel (James S. Wolf, NASA TN D-5266, Lewis Research Center)
id: NTRS 19690017683
url: https://ntrs.nasa.gov/api/citations/19690017683/downloads/19690017683.pdf
year: 1969
kind: report
license: public domain (NASA)
clemmer-2006-nio-ysz:
title: The Processing and Characterization of Porous Ni/YSZ and NiO/YSZ Composites used in Solid Oxide Fuel Cell Applications (Ryan Clemmer, University of Waterloo)
id: UWSpace handle 10012/2883
url: https://uwspace.uwaterloo.ca/handle/10012/2883
year: 2006
kind: paper
license: not stated on the repository page
carex-nickel:
title: CAREX Canada, Nickel profile
id: CAREX Canada nickel profile
url: https://www.carexcanada.ca/?p=9614
year: 2026
kind: web
license: not stated
usgs-mcs2026-nickel:
title: Mineral Commodity Summaries 2026, Nickel
id: USGS MCS 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-nickel.pdf
year: 2026
kind: report
license: public domain (USGS)
usgs-crit2025:
title: About the 2025 List of Critical Minerals (USGS, final list of 60 minerals)
id: Final 2025 List of Critical Minerals
url: https://www.usgs.gov/programs/mineral-resources-program/science/about-2025-list-critical-minerals
year: 2025
kind: web
license: public domain (USGS)
niosh-npg-nickel:
title: NIOSH Pocket Guide to Chemical Hazards, Nickel metal and other compounds (as Ni)
id: NIOSH NPG entry npgd0445; CAS 7440-02-0 (metal)
url: https://www.cdc.gov/niosh/npg/npgd0445.html
year: 2026
kind: handbook
license: public domain (CDC)
license: CC-BY-4.0
updated: '2026-10-26'
review:
status: draft
method: assistant
checked_values: 13
unreachable: 4
caveats: 6
note: 'Read by an AI assistant on 2026-10-26 from the pages and PDFs fetched in that run. Two MDPI papers (the SOFC redox review and the p-type Ni1-xO film paper) returned HTTP 403, and the IARC Volume 100C PDF did not download. The PubChem experimental-properties page returned a verification screen. The Solaronix SDS is for a paste, not pure NiO. The melting point comes from one reseller SDS. Caveats: the Membranes review and the Coatings paper are not used; the battery-precursor use is not sourced; the alloy-scale statements rest on the NASA report and a search snippet only.'
story:
recipe:
line: NiO is a 1:1 compound of nickel and oxygen. It crystallises in the face-centred cubic rock-salt structure (space group Fm3m), with a lattice constant of 4.169 Å at 298 K. Simple rock-salt structure is one reason the 2024 review gives for its use as a p-type transparent conductor.
parts:
- name: Nickel
symbol: Ni
role: The metal cation. Ni(II) ions sit in the rock-salt lattice with oxygen as the counter-ion.
- name: Oxygen
symbol: O
role: The anion. Oxygen forms the other half of the rock-salt lattice with nickel.
risk_groups:
- title: For people
level: 1
verdict: Cancer risk by inhalation; skin sensitiser
lead: The supplier safety data sheets classify nickel oxide as a Danger-level carcinogen and skin sensitiser. IARC places nickel compounds in Group 1.
points:
- label: Inhalation
line: The Sigma-Aldrich SDS gives H350 (may cause cancer) and H372 (organ damage from repeated exposure). The paste SDS gives H350i (cancer by inhalation).
- label: Dust limits
line: OSHA PEL 1 mg/m3, NIOSH REL 0.015 mg/m3 (potential carcinogen), and ACGIH TLV 0.2 mg/m3 are the workplace limits printed in the SDS.
- label: Skin
line: H317 means it can cause an allergic skin reaction.
- title: If the oxide is heated or cycled
lead: High-temperature oxidation and redox cycling change the stress and the volume of nickel-based parts.
points:
- label: Scale stress
line: On nickel at 1000 °C in oxygen, the NiO scale carries a compressive stress of about 10 MN/m2.
- label: Anode cycling
line: In Ni/YSZ composites, nickel expands when it oxidises, so the nickel loading has to stay in a window.
- title: Handling and storage
points:
- label: Dust
line: Avoid dust formation and provide exhaust ventilation. Clean up spills without creating dust.
- label: Storage
line: Handle and store under inert gas, in a dry place, as the Sigma-Aldrich SDS says.
why: 'Nickel oxide is a simple rock-salt oxide and the p-type counterpart to n-type transparent oxides such as zinc oxide. Its record in the sources read is in three places: sputtered films that conduct as p-type layers (7.2 and 9.09 S/cm, with 40 to 69 percent transmittance), porous Ni/YSZ and NiO/YSZ composites studied as solid oxide fuel cell anodes, and a NiO scale on nickel that builds a compressive stress of about 10 MN/m2 at 1000 °C. Its weak point is the hazard: the SDS classes it as a carcinogen and IARC places nickel compounds in Group 1. No flight or space-exposure data for NiO was found.'
uses:
- where: Transparent p-type layers
line: The 2024 review calls NiO the first p-type transparent conducting oxide. It is mostly used in transparent p-n junctions and thin-film transistors.
- where: Solid oxide fuel cell anodes
line: A 2006 Waterloo thesis studied porous Ni/YSZ and NiO/YSZ composites with nickel loadings from 4 to 77 vol%, and found the nickel loading must stay in a window to keep conductivity and avoid thermal mismatch with the electrolyte.
- where: Oxide scale on nickel and nickel alloys
line: A NiO scale on nickel at 1000 °C in oxygen carries a compressive stress of about 10 MN/m2. The NASA report expects its results to apply to nickel-base alloys.
can_do:
- label: p-type conduction
value: 7.2 S/cm at 110 nm
line: A 110 nm sputtered NiO film on glass conducts at 7.2 S/cm with 40 percent average transmittance.
- label: Higher conductivity film
value: 9.09 S/cm at 100 nm
line: An RF-sputtered 100 nm NiO film reached 9.09 S/cm, 69 percent transmittance and 6.12 cm2/V-s Hall mobility.
- label: Crystal cell
value: 4.169 Å cubic lattice
line: The rock-salt cell has a lattice constant of 4.169 Å at 298 K from X-ray refinement.
- label: Scale stress
value: about 10 MN/m2 at 1000 °C
line: Nickel oxide grown on nickel in oxygen at 1000 °C carries a grain-boundary pressure of about 10 MN/m2.
compare: 'Compared with zinc oxide, nickel oxide melts at a higher temperature and is denser, as the compare rows show. Its sputtered-film conductivity (7.2 to 9.09 S/cm) is for an undoped p-type film, so it is not directly comparable with the doped n-type zinc oxide films. The main difference is the hazard: zinc oxide is classed only as an aquatic hazard in its SDS, while nickel oxide carries a carcinogen classification.'
compare_rows:
- label: Melting point
benchmark: melting_point
- label: Density
benchmark: density
- label: Band gap
benchmark: band_gap
handling:
- Avoid dust and use exhaust ventilation.
- Handle and store under inert gas in a dry place.
- Treat it as a carcinogen and keep exposure within the OSHA, NIOSH and ACGIH limits printed in the SDS.
good_for:
- Undoped p-type transparent layers in research devices, at 7.2 to 9.09 S/cm in sputtered films.
- Nickel-based solid oxide fuel cell anode work, where the NiO/YSZ composite is the starting material.
- Studying oxide scale growth on nickel at high temperature, where the scale stress is about 10 MN/m2 at 1000 °C.
watch_out:
- 'The carcinogen classification: H350 in the Sigma-Aldrich SDS, H350i in the paste SDS, and IARC Group 1 for nickel compounds.'
- Volume change of nickel on oxidation in anodes, and the scale growth stress on nickel.
- Hazard classes differ between the SDS sheets read, and the PubChem summary is mixed.
verdict: Nickel oxide is a simple, well-characterised p-type oxide, with film conductivity of about 7 to 9 S/cm in the sources read. Its carcinogen classification and dust hazard make it a controlled material. It has no flight record, and the battery-precursor use is not backed by a source read in this run, so it is listed as a gap.
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.