Inconel 625 IN625 (UNS N06625)
Nickel-chromium-molybdenum-niobium solid-solution alloy: 58.0 min Ni, 20.0 to 23.0 Cr, 8.0 to 10.0 Mo, 3.15 to 4.15 Nb plus Ta, 5.0 max Fe, 1.0 max Co (if determined), 0.50 max Mn, 0.50 max Si, 0.40 max Al, 0.40 max Ti, 0.10 max C, 0.015 max P, 0.015 max S (wt%)
Also known as UNS N06625, EN 2.4856, ISO NW6625, ASTM B 443, ASTM B 444, ASTM B 446 · 14 more
Inconel 625 (UNS N06625, W.Nr.
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Recipe, share of the weight
- Ni minimum (the matrix)Nickel
- Cr 20 to 23%Chromium
- Mo 8 to 10%Molybdenum
- Nb 3.15 to 4.15%Niobium plus tantalum
- Fe 5.0 maximumIron
- Co 1.0 maximum, if determinedCobalt
- C 0.10, Mn 0.50, Si 0.50, Al 0.40, Ti 0.40, P 0.015 and S 0.015 maximum (wt%)Minor elements
Best for
Corrosion-resistant parts that also need strength and good weldability, such as chemical plant, marine hardware, aerospace ducting and rocket tubing
Weakest at
Long exposure near 1200 F hardens the annealed alloy and cuts its room-temperature elongation from 54 to 30 percent after 2000 hours
Risk at a glance
- People Moderate. Solid metal flagged by the nickel record; powder is Danger
- If it fails High. Notch sensitivity in fatigue
- Corrosion Moderate. Hardens on exposure near 1200 F and loses ductility; no embrittling sigma phase was found after 1000 to 1800 F exposure (Special Metals).
Quick facts: IN625 (UNS N06625)
| Property | Value | Basis |
|---|---|---|
| Density | 8.44 g/cm³ | 1 sourced value |
| Yield strength | 290 to 655 MPa | 6 sourced values across conditions |
| Tensile strength | 724 to 1,034 MPa | 6 sourced values across conditions |
| Young's modulus | 205 to 208 GPa | 2 sourced values across conditions |
| Thermal conductivity | 9.8 W/(m·K) | 1 sourced value |
| Thermal expansion (CTE) | 12.8 to 14.8 ppm/K | 2 sourced values across conditions |
| Melting point | 1,290 to 1,350 °C | 1 sourced value |
| Specific heat | 410 J/(kg·K) | 1 sourced value |
| Electrical resistivity | 0.0000013 Ω·m | 1 sourced value |
| Maximum service temperature | 982 °C | 1 sourced value |
What is the density of Inconel 625?
Inconel 625 has a density of 8.44 g/cm³. The source and test conditions are listed in the properties table on this page.
What is the thermal conductivity of Inconel 625?
Inconel 625 has a thermal conductivity of 9.8 W/(m·K). The source and test conditions are listed in the properties table on this page.
What is the coefficient of thermal expansion of Inconel 625?
Inconel 625 has a coefficient of thermal expansion of 12.8 to 14.8 ppm/K. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the melting point of Inconel 625?
Inconel 625 has a melting point of 1,290 to 1,350 °C. The source and test conditions are listed in the properties table on this page.
What is the yield strength of Inconel 625?
Inconel 625 has a yield strength of 290 to 655 MPa. The range covers 6 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What are the other names and codes for Inconel 625?
Inconel 625 is also written as UNS N06625, EN 2.4856, ISO NW6625, ASTM B 443, ASTM B 444, ASTM B 446. Each code is printed in the source listed beside it in the designations table.
What is Inconel 625 used for?
Uses recorded in the sources include Thrust-chamber tubing for rocket engines, fuel and hydraulic line tubing, and engine exhaust systems; Aircraft ducting systems, resistance-welded honeycomb structures housing engine controls, and turbine shroud rings; Heat-exchanger tubing in environmental control systems.
Why it exists
Inconel 625 was first developed as a steam-line piping material and has since spread to chemical processing, marine and nuclear equipment and aerospace ducting (Wikipedia; ATI). Its strength comes from molybdenum and niobium stiffening the nickel-chromium matrix, so it needs no precipitation-hardening step (Special Metals). That combination gives resistance to a wide range of corrosive media, including chloride stress-corrosion cracking, and good oxidation resistance (Special Metals; ATI).
Where it's used
Rocket engines and fuel lines
Special Metals lists thrust-chamber tubing for rocket engines, fuel and hydraulic line tubing, engine exhaust systems and combustion-system transition liners among its aerospace uses.
Aircraft structures and ducting
Aircraft ducting systems, resistance-welded honeycomb structures housing engine controls, and turbine shroud rings are named in the datasheet. ATI says the alloy is widely used in aerospace for airframe and jet engine applications.
Heat exchangers in environmental control systems
Special Metals lists heat-exchanger tubing in environmental control systems among its aerospace uses.
Chemical plant and marine service
Special Metals names bubble caps, tubing, reaction vessels, distillation columns, heat exchangers and valves for chemical processing, and wire rope for mooring cables, propeller blades and sheathing for undersea cables for marine service.
Recipe
Nickel-chromium-molybdenum-niobium solid-solution alloy: 58.0 min Ni, 20.0 to 23.0 Cr, 8.0 to 10.0 Mo, 3.15 to 4.15 Nb plus Ta, 5.0 max Fe, 1.0 max Co (if determined), 0.50 max Mn, 0.50 max Si, 0.40 max Al, 0.40 max Ti, 0.10 max C, 0.015 max P, 0.015 max S (wt%)
Inconel 625 is a solid-solution nickel-chromium-molybdenum-niobium alloy, made by vacuum induction melting followed by electroslag remelting (ATI TDS). Special Metals gives the limiting composition in weight percent: at least 58 percent nickel, 20 to 23 percent chromium, 8 to 10 percent molybdenum, 3.15 to 4.15 percent niobium plus tantalum, and up to 5 percent iron, with small maximum limits on the other elements.
| Ingredient | Share of the weight | What it does |
|---|---|---|
| Nickel Ni | minimum (the matrix) | Matrix of the alloy, a face-centred-cubic solid solution |
| Chromium Cr | 20 to 23% | Gives resistance to oxidising chemicals and to oxidation and scaling at high temperature |
| Molybdenum Mo | 8 to 10% | Stiffens the matrix and makes the alloy very resistant to pitting and crevice corrosion |
| Niobium plus tantalum Nb | 3.15 to 4.15% | Stiffens the matrix, which is the main strengthening effect, and stabilises the alloy against sensitisation during welding |
| Iron Fe | 5.0 maximum | Residual element, limited to 5.0 percent |
| Cobalt Co | 1.0 maximum, if determined | Residual element |
| Minor elements | C 0.10, Mn 0.50, Si 0.50, Al 0.40, Ti 0.40, P 0.015 and S 0.015 maximum (wt%) | Residual limits. The datasheet says precipitation-hardening treatments are not required. |
Weight shares are as printed in the sources.
What it can do
Strength in the annealed grade
Annealed (grade 1) rod, bar and plate give 60 to 95 ksi yield and 120 to 150 ksi tensile strength at room temperature (Special Metals Table 5, composite ranges).
Lower strength in the solution-annealed grade
Solution-annealed (grade 2) rod, bar and plate give 42 to 60 ksi yield and 105 to 130 ksi tensile strength, so the two grades differ in strength (Table 5).
Stiffness
Young modulus is 207.5 GPa for the annealed grade and 204.8 GPa for the solution-annealed grade at 21 C (Table 4).
Oxidation at high temperature
The datasheet gives service up to 1800 F (982 C), and ATI rates oxidation resistance as excellent up to 2,000 F (1,093 C).
Corrosion in mild and severe media
Almost no attack in the atmosphere, fresh and sea water, neutral salts and alkaline media, and freedom from chloride-ion stress-corrosion cracking (Special Metals).
How it compares
Compare with [Inconel 718](/profiles/inconel-718/), the age-hardened sibling. Its strength comes from precipitates formed in heat treatment, while Inconel 625 is solid-solution strengthened and the Special Metals datasheet says no precipitation-hardening treatment is required. The 718 profile carries its own precipitation and heat-treatment data.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | IN625 (UNS N06625) | IN718 (UNS N07718) | FeNi36 | Ni-Mo | C-22 | C-276 (UNS N10276) | X (UNS N06002) | UNS N07214 | H230 (UNS N06230) | UNS N08800 | Alloy 825 (UNS N08825) | Alloy 600 (UNS N06600, W.Nr. 2.4816) | Alloy 601 | Alloy 617 | X-750 (UNS N07750) | Fe-Ni-Co | Alloy 400 (UNS N04400) | K-500 | Ni | Ni3Al, NiAl | NiBe2 | Ni-alloys | UNS N07090 (W. Nr. 2.4632) | UNS N07001 |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Thermal behavior and safety | ||||||||||||||||||||||||
| melting point | 1290 to 1350 °C2 | 1260 °C | 1427 °C | 1370 to 1418 °C | 1357 to 1399 °C | 1323 to 1371 °C | 1260 to 1355 °C | 1355 to 1400 °C | 1301 to 1371 °C | 1357 to 1385 °C | 1370 to 1400 °C | 1354 to 1413 °C | 1360 to 1411 °C | 1330 to 1380 °C | 1393 to 1427 °C | 1450 °C | 1300 to 1350 °C | 1315 to 1350 °C | 1455 °C | no data | 1195 to 1325 °C | 1425 °C | 1370 °C | 1330 to 1360 °C |
| specific heat | 410 J/(kg·K)3 | 435 J/kg °C | 515 J/(kg·K) | 373 J/kg.°C | 410 J/(kg·K) | 427 J/kg.°C | 486 J/(kg·K) | 452 J/kg-°C | 397 J/kg·°C | 460 J/kg·°C | 440 J/(kg·K) | 444 J/kg °C | 448 J/(kg·K) | 419 J/(kg·K) | 0.103 Btu/lb/°F | 500 J/(kg. K) | 427 J/kg°C | 419 J/kg °C | 456 J/(kg·K) | no data | no data | 500 J/(kg·K) | 446 J/(kg·K) | no data |
| Thermal conductivity | 9.8 W/m°C5 | 79 BTU·in/ft²·h·°F | 72.85 Btu·in/(hr·ft²·°F) | 11.2 W/m.°C | 10.1 W/(m·K) | 10.5 W/m.°C | 9.2 W/(m·K) | 12 W/m-°C | 8.9 W/(m·°C) | 11.5 W/m°C | 11.1 W/(m·K) | 14.9 W/(m·K) | 11.2 W/(m·K) | 13.4 W/(m·K) | 83 Btu/in./hr/sq ft/°F | 17.5 W/m °K | 22 W/m°C | 17.5 W/m °C | 70.3 W/(m·K) | no data | 48 W/(m·K) | 13 W/(m·K) | 11.47 W/(m·K) | 19.1 W/(m·°C) |
| Thermal conductivity | 25.2 W/m°C6 | 79 BTU·in/ft²·h·°F | 72.85 Btu·in/(hr·ft²·°F) | 11.2 W/m.°C | 10.1 W/(m·K) | 10.5 W/m.°C | 9.2 W/(m·K) | 12 W/m-°C | 8.9 W/(m·°C) | 11.5 W/m°C | 11.1 W/(m·K) | 14.9 W/(m·K) | 11.2 W/(m·K) | 13.4 W/(m·K) | 83 Btu/in./hr/sq ft/°F | 17.5 W/m °K | 22 W/m°C | 17.5 W/m °C | 70.3 W/(m·K) | no data | 48 W/(m·K) | 13 W/(m·K) | 11.47 W/(m·K) | 19.1 W/(m·°C) |
| Physical and electrical | ||||||||||||||||||||||||
| Density | 8.44 g/cm³1 | 0.297 lb/in3 | 8.05 g/cm³ | 9.22 g/cm³ | 8.69 g/cm³ | 8.89 g/cm³ | 8.22 g/cm³ | 8.05 g/cm³ | 8.97 g/cm³ | 7.94 g/cm³ | 8.14 g/cm³ | 0.306 lb/in3 | 8.11 Mg/m3 | 8.36 g/cm³ | 8.28 g/cm³ | 8.36 g/cm³ | 8.8 g/cm³ | 8.45 g/cm³ | 8.89 g/cm³ | 7.5 g/cm³ | 8.27 g/cm³ | 8.2 g/cm³ | 8.18 g/cm³ | 8.19 g/cm³ |
| electrical resistivity | 129 µΩ-cm7 | 725 ohm circ mil/ft | 84 µΩ·cm | 1.37 μohm.m | 1.14 µΩ·m | 1.23 μohm.m | 114.8 µohm-cm | 135.9 µohm-cm | 125 µohm-m | 0.989 µΩ·m | 112 µΩ·cm | 1.03 µΩ·m | 1.18 µΩ·m | 1.22×10^-4 Ω·cm | 731 ohm circ mil/ft | 49 μΩcm | 0.511 µΩ·m | 0.615 µΩ·m | 0.096 µΩ·m | no data | < 28.7 µΩ·cm | 45 µΩ·cm | 1.18 µΩ·m | 1.24 µΩ·m |
| Temperature behavior | ||||||||||||||||||||||||
| curie temperature | < -196 °C4 | -112 °C | 279 °C | no data | no data | no data | no data | no data | no data | -115 °C | < -196 °C | -124 °C | no data | no data | no data | 435 °C | 21 to 49 °C | -65 °C | 360 °C | no data | no data | 450 °C | no data | no data |
| Other measurements | ||||||||||||||||||||||||
| Thermal expansion (CTE) | 12.8 ppm/°C8 | 8.91 ppm/°F | 1.3 ppm/K | 10.6 μm/m.°C | 12.4 ppm/K | 11.2 μm/m.°C | 13.9 µm/(m·K) | 14.6 µm/m-°C | 11.8 ppm/K | 14.4 µm/m/°C | 13.9 ppm/K | 10.4 ppm/K | 13.75 µm/m/°C | 11.6 µm/(m·K) | 7 10-6 in./in./°F | 5.86 10-6/°C | 14.2 µm/m°C | 13.7 10-6/°C | 13.3 ppm/K | no data | 14.5 ppm/K | 8 ppm/K | 12.7 µm/(m·K) | 14.3 µm/m·°C |
| Thermal expansion (CTE) | 14.8 ppm/°C9 | 8.91 ppm/°F | 1.3 ppm/K | 10.6 μm/m.°C | 12.4 ppm/K | 11.2 μm/m.°C | 13.9 µm/(m·K) | 14.6 µm/m-°C | 11.8 ppm/K | 14.4 µm/m/°C | 13.9 ppm/K | 10.4 ppm/K | 13.75 µm/m/°C | 11.6 µm/(m·K) | 7 10-6 in./in./°F | 5.86 10-6/°C | 14.2 µm/m°C | 13.7 10-6/°C | 13.3 ppm/K | no data | 14.5 ppm/K | 8 ppm/K | 12.7 µm/(m·K) | 14.3 µm/m·°C |
| elastic modulus | 207.5 GPa10 | 29 ksi x 10^3 | 140 GPa | 216 GPa | 206 GPa | 205 GPa | 205 GPa | 218 GPa | 209 GPa | 196.5 GPa | 196 GPa | 214 GPa | 206.5 GPa | 211 GPa | 31 10^3 ksi | 138 kN/mm2 | 26 10^3 ksi | 179 GPa | 205 GPa | 200 GPa | 195 to 210 GPa | no data | 204 GPa | 211 GPa |
| elastic modulus | 204.8 GPa11 | 29 ksi x 10^3 | 140 GPa | 216 GPa | 206 GPa | 205 GPa | 205 GPa | 218 GPa | 209 GPa | 196.5 GPa | 196 GPa | 214 GPa | 206.5 GPa | 211 GPa | 31 10^3 ksi | 138 kN/mm2 | 26 10^3 ksi | 179 GPa | 205 GPa | 200 GPa | 195 to 210 GPa | no data | 204 GPa | 211 GPa |
| elastic modulus | 147.5 GPa12 | 29 ksi x 10^3 | 140 GPa | 216 GPa | 206 GPa | 205 GPa | 205 GPa | 218 GPa | 209 GPa | 196.5 GPa | 196 GPa | 214 GPa | 206.5 GPa | 211 GPa | 31 10^3 ksi | 138 kN/mm2 | 26 10^3 ksi | 179 GPa | 205 GPa | 200 GPa | 195 to 210 GPa | no data | 204 GPa | 211 GPa |
| elastic modulus | 148.2 GPa13 | 29 ksi x 10^3 | 140 GPa | 216 GPa | 206 GPa | 205 GPa | 205 GPa | 218 GPa | 209 GPa | 196.5 GPa | 196 GPa | 214 GPa | 206.5 GPa | 211 GPa | 31 10^3 ksi | 138 kN/mm2 | 26 10^3 ksi | 179 GPa | 205 GPa | 200 GPa | 195 to 210 GPa | no data | 204 GPa | 211 GPa |
| poissons ratio | 0.278 -14 | 0.294 - | no data | no data | no data | 0.31 - | 0.32 - | no data | 0.31 - | 0.339 - | no data | 0.324 - | 0.272 - | no data | 0.29 - | no data | 0.32 - | no data | no data | no data | 0.3 - | no data | no data | no data |
| poissons ratio | 0.312 -15 | 0.294 - | no data | no data | no data | 0.31 - | 0.32 - | no data | 0.31 - | 0.339 - | no data | 0.324 - | 0.272 - | no data | 0.29 - | no data | 0.32 - | no data | no data | no data | 0.3 - | no data | no data | no data |
| ultimate tensile strength | 120 to 150 ksi16 | 201 ksi | 65 ksi | 862 MPa | 690 to 950 MPa | 792 MPa | 760 MPa | 975 MPa | 837 MPa | 590 MPa | 662 MPa | 550 to 690 MPa | 675 MPa | 710 MPa | > 165 ksi | 450 to 585 N/mm2 | 75 to 90 ksi | 621 to 758 MPa | 380 to 520 MPa | 2300 MPa | 660 to 900 MPa | 500 MPa | 1175 MPa | 1027 MPa |
| yield strength | 60 to 95 ksi17 | 171 ksi | 40 ksi | 421 MPa | > 310 MPa | 356 MPa | 340 MPa | 577 MPa | 417 MPa | 250 MPa | 338 MPa | 170 to 345 MPa | 292 MPa | 340 MPa | > 105 ksi | > 200 N/mm2 | 25 to 50 ksi | 276 to 414 MPa | 105 to 210 MPa | no data | 280 to 480 MPa | 280 MPa | 752 MPa | 586 MPa |
| elongation | 30 to 60 %18 | 26 % | 35 % | 53 % | > 45 % | 61 % | 48.9 % | 37.3 % | 47.3 % | 17 % | 45 % | 35 to 55 % | 46 % | 62 % | > 20 % | > 25 % | 35 to 60 % | 20 to 35 % | 40 to 55 % | no data | > 30 % | 35 % | 30 % | 43 % |
| ultimate tensile strength | 105 to 130 ksi19 | 201 ksi | 65 ksi | 862 MPa | 690 to 950 MPa | 792 MPa | 760 MPa | 975 MPa | 837 MPa | 590 MPa | 662 MPa | 550 to 690 MPa | 675 MPa | 710 MPa | > 165 ksi | 450 to 585 N/mm2 | 75 to 90 ksi | 621 to 758 MPa | 380 to 520 MPa | 2300 MPa | 660 to 900 MPa | 500 MPa | 1175 MPa | 1027 MPa |
| yield strength | 42 to 60 ksi20 | 171 ksi | 40 ksi | 421 MPa | > 310 MPa | 356 MPa | 340 MPa | 577 MPa | 417 MPa | 250 MPa | 338 MPa | 170 to 345 MPa | 292 MPa | 340 MPa | > 105 ksi | > 200 N/mm2 | 25 to 50 ksi | 276 to 414 MPa | 105 to 210 MPa | no data | 280 to 480 MPa | 280 MPa | 752 MPa | 586 MPa |
| elongation | 40 to 65 %21 | 26 % | 35 % | 53 % | > 45 % | 61 % | 48.9 % | 37.3 % | 47.3 % | 17 % | 45 % | 35 to 55 % | 46 % | 62 % | > 20 % | > 25 % | 35 to 60 % | 20 to 35 % | 40 to 55 % | no data | > 30 % | 35 % | 30 % | 43 % |
| ultimate tensile strength | 120 to 150 ksi22 | 201 ksi | 65 ksi | 862 MPa | 690 to 950 MPa | 792 MPa | 760 MPa | 975 MPa | 837 MPa | 590 MPa | 662 MPa | 550 to 690 MPa | 675 MPa | 710 MPa | > 165 ksi | 450 to 585 N/mm2 | 75 to 90 ksi | 621 to 758 MPa | 380 to 520 MPa | 2300 MPa | 660 to 900 MPa | 500 MPa | 1175 MPa | 1027 MPa |
| yield strength | 60 to 90 ksi23 | 171 ksi | 40 ksi | 421 MPa | > 310 MPa | 356 MPa | 340 MPa | 577 MPa | 417 MPa | 250 MPa | 338 MPa | 170 to 345 MPa | 292 MPa | 340 MPa | > 105 ksi | > 200 N/mm2 | 25 to 50 ksi | 276 to 414 MPa | 105 to 210 MPa | no data | 280 to 480 MPa | 280 MPa | 752 MPa | 586 MPa |
| ultimate tensile strength | 143.5 ksi24 | 201 ksi | 65 ksi | 862 MPa | 690 to 950 MPa | 792 MPa | 760 MPa | 975 MPa | 837 MPa | 590 MPa | 662 MPa | 550 to 690 MPa | 675 MPa | 710 MPa | > 165 ksi | 450 to 585 N/mm2 | 75 to 90 ksi | 621 to 758 MPa | 380 to 520 MPa | 2300 MPa | 660 to 900 MPa | 500 MPa | 1175 MPa | 1027 MPa |
| yield strength | 83.6 ksi25 | 171 ksi | 40 ksi | 421 MPa | > 310 MPa | 356 MPa | 340 MPa | 577 MPa | 417 MPa | 250 MPa | 338 MPa | 170 to 345 MPa | 292 MPa | 340 MPa | > 105 ksi | > 200 N/mm2 | 25 to 50 ksi | 276 to 414 MPa | 105 to 210 MPa | no data | 280 to 480 MPa | 280 MPa | 752 MPa | 586 MPa |
| ultimate tensile strength | 116 ksi26 | 201 ksi | 65 ksi | 862 MPa | 690 to 950 MPa | 792 MPa | 760 MPa | 975 MPa | 837 MPa | 590 MPa | 662 MPa | 550 to 690 MPa | 675 MPa | 710 MPa | > 165 ksi | 450 to 585 N/mm2 | 75 to 90 ksi | 621 to 758 MPa | 380 to 520 MPa | 2300 MPa | 660 to 900 MPa | 500 MPa | 1175 MPa | 1027 MPa |
| yield strength | 50 ksi27 | 171 ksi | 40 ksi | 421 MPa | > 310 MPa | 356 MPa | 340 MPa | 577 MPa | 417 MPa | 250 MPa | 338 MPa | 170 to 345 MPa | 292 MPa | 340 MPa | > 105 ksi | > 200 N/mm2 | 25 to 50 ksi | 276 to 414 MPa | 105 to 210 MPa | no data | 280 to 480 MPa | 280 MPa | 752 MPa | 586 MPa |
| ultimate tensile strength | 146.5 ksi28 | 201 ksi | 65 ksi | 862 MPa | 690 to 950 MPa | 792 MPa | 760 MPa | 975 MPa | 837 MPa | 590 MPa | 662 MPa | 550 to 690 MPa | 675 MPa | 710 MPa | > 165 ksi | 450 to 585 N/mm2 | 75 to 90 ksi | 621 to 758 MPa | 380 to 520 MPa | 2300 MPa | 660 to 900 MPa | 500 MPa | 1175 MPa | 1027 MPa |
| yield strength | 106.5 ksi29 | 171 ksi | 40 ksi | 421 MPa | > 310 MPa | 356 MPa | 340 MPa | 577 MPa | 417 MPa | 250 MPa | 338 MPa | 170 to 345 MPa | 292 MPa | 340 MPa | > 105 ksi | > 200 N/mm2 | 25 to 50 ksi | 276 to 414 MPa | 105 to 210 MPa | no data | 280 to 480 MPa | 280 MPa | 752 MPa | 586 MPa |
| elongation | 54 %30 | 26 % | 35 % | 53 % | > 45 % | 61 % | 48.9 % | 37.3 % | 47.3 % | 17 % | 45 % | 35 to 55 % | 46 % | 62 % | > 20 % | > 25 % | 35 to 60 % | 20 to 35 % | 40 to 55 % | no data | > 30 % | 35 % | 30 % | 43 % |
| elongation | 30 %31 | 26 % | 35 % | 53 % | > 45 % | 61 % | 48.9 % | 37.3 % | 47.3 % | 17 % | 45 % | 35 to 55 % | 46 % | 62 % | > 20 % | > 25 % | 35 to 60 % | 20 to 35 % | 40 to 55 % | no data | > 30 % | 35 % | 30 % | 43 % |
| fatigue strength | 90000 psi32 | no data | no data | no data | no data | no data | no data | no data | no data | 214 MPa | no data | 268.9 MPa | no data | no data | no data | no data | no data | no data | no data | no data | 586 to 655 MPa | no data | no data | no data |
| fatigue strength | 35000 psi33 | no data | no data | no data | no data | no data | no data | no data | no data | 214 MPa | no data | 268.9 MPa | no data | no data | no data | no data | no data | no data | no data | no data | 586 to 655 MPa | no data | no data | no data |
| Maximum service temperature | 982 °C34 | 1300 °F | no data | no data | no data | 677 °C | no data | 1260 °C | no data | no data | no data | no data | 1000 °C | no data | 1200 °F | no data | no data | 650 °C | no data | 1373 K | no data | no data | no data | 650 °C |
| ultimate tensile strength | > 120 ksi35 | 201 ksi | 65 ksi | 862 MPa | 690 to 950 MPa | 792 MPa | 760 MPa | 975 MPa | 837 MPa | 590 MPa | 662 MPa | 550 to 690 MPa | 675 MPa | 710 MPa | > 165 ksi | 450 to 585 N/mm2 | 75 to 90 ksi | 621 to 758 MPa | 380 to 520 MPa | 2300 MPa | 660 to 900 MPa | 500 MPa | 1175 MPa | 1027 MPa |
| yield strength | > 60 ksi36 | 171 ksi | 40 ksi | 421 MPa | > 310 MPa | 356 MPa | 340 MPa | 577 MPa | 417 MPa | 250 MPa | 338 MPa | 170 to 345 MPa | 292 MPa | 340 MPa | > 105 ksi | > 200 N/mm2 | 25 to 50 ksi | 276 to 414 MPa | 105 to 210 MPa | no data | 280 to 480 MPa | 280 MPa | 752 MPa | 586 MPa |
| elongation | > 30 %37 | 26 % | 35 % | 53 % | > 45 % | 61 % | 48.9 % | 37.3 % | 47.3 % | 17 % | 45 % | 35 to 55 % | 46 % | 62 % | > 20 % | > 25 % | 35 to 60 % | 20 to 35 % | 40 to 55 % | no data | > 30 % | 35 % | 30 % | 43 % |
Why choose it, and why not
Good for
- Corrosion-resistant parts that must also carry strength, such as chemical plant equipment, marine hardware and sea-water service (Special Metals).
- Hot ducting and exhaust parts up to 1800 F (982 C) where oxidation resistance matters (Special Metals; ATI).
- Welded assemblies that need corrosion resistance matched to the base alloy (Special Metals).
Watch out for
- Long exposure near 1200 F hardens the annealed alloy and drops room-temperature elongation from 54 to 30 percent after 2000 hours (Special Metals Table 6).
- The annealed (grade 1) and solution-annealed (grade 2) grades differ in strength, so the grade must be stated on any design basis (Special Metals; ATI).
- Strength ranges are composites for product sizes up to 4 in and are not specification values (Special Metals).
- Notched fatigue strength is far below smooth fatigue strength, 35,000 psi against 90,000 psi (Special Metals).
- The corrosion entries are qualitative. No corrosion rate or critical pitting temperature was read in this run.
Inconel 625 is a corrosion-resistant solid-solution alloy for strength up to 1800 F. Its annealed and solution-annealed grades differ in strength, so state the grade for each design, and keep long exposures near 1200 F in mind.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Other names and standards
The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.
| System | Codes |
|---|---|
| UNS | N06625 |
| EN | 2.4856, 10095 |
| ISO | NW6625 |
| ASTM | B 443, B 444, B 446 |
| AMS | 5599, 5666, 5837 |
| MIL | N-24687, MIL-DTL-24799 |
| NACE | MR-01-75 |
| Trade name | INCONEL alloy 625, ATI 625, Haynes 625, Nickelvac 625, Nicrofer 6020, Altemp 625, Chronin 625 |
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Density | Table 2, Physical Constants, Density, printed as 0.305 lb/cu in and 8.44 gram/cc; the gram/cc value is kept | basis datasheet physical constant, no test temperature printedunit in source gram/cc (0.305 lb/cu in printed alongside) | — |
| 2 | melting point | Table 2, metric row printed as 1290-1350 C; the ATI TDS prints 1,288 to 1,343 C (2,350 to 2,450 F), and the Special Metals range is kept here | basis melting range as printed in Table 2 (2350 to 2460 F) | — |
| 3 | specific heat | Table 2, metric value in parentheses; the datasheet marks the row as calculated (footnote a) | basis at 70 F (21 C); printed as 0.098 Btu/lb Funit in source J/kg °C | — |
| 4 | curie temperature | Table 2, Curie Temperature, C row; the metric row has no less-than sign, so the value is recorded as an upper bound | basis printed as less than -320 F; metric value -196 C | — |
| 5 | Thermal conductivity | Table 3, Thermal Conductivity, metric column; the same row prints 68 Btu·in/ft²·h·°F at 70 F | basis at 21 C (70 F); material annealed 2100 F for 1 h (footnote c); measured at Battelle (footnote b) | — |
| 6 | Thermal conductivity | Table 3, Thermal Conductivity, metric column, row 982 C (1800 F) | basis at 982 C (1800 F); material annealed 2100 F for 1 h (footnote c) | — |
| 7 | electrical resistivity | Table 3, Electrical Resistivity, metric column; the imperial column prints 776 ohm circ mil/ft at 70 F | basis at 21 C (70 F); material annealed 2100 F for 1 h (footnote c) | — |
| 8 | Thermal expansion (CTE) | Table 3, Mean Linear Expansion, metric column (µm/µm·°C is the same unit as ppm/°C); the imperial column prints 7.1 x 10^-6 in/in·°F at 200 F | basis mean linear expansion from 21 C (70 F) to 93 C (200 F), footnote amaterial not stated in the datasheetunit in source µm/µm·°C | — |
| 9 | Thermal expansion (CTE) | Table 3, Mean Linear Expansion, metric column, row 649 C; the imperial column prints 8.2 x 10^-6 in/in·°F at 1200 F | basis mean linear expansion from 21 C (70 F) to 649 C (1200 F), footnote amaterial not stated in the datasheetunit in source µm/µm·°C | — |
| 10 | elastic modulus | Table 4, Modulus of Elasticity, tension, GPa column; the imperial column prints 30.1 x 10^3 ksi for the same row | condition annealed (grade 1)temperature 21 C (70 F)basis tension modulus, measured dynamically on 3/4 in hot-rolled rod (footnote a) | — |
| 11 | elastic modulus | Table 4, Modulus of Elasticity, tension, GPa column; the imperial column prints 29.7 x 10^3 ksi for the same row | condition solution-annealed (grade 2; Special Metals calls it solution-treated)temperature 21 C (70 F)basis tension modulus, measured dynamically on 3/4 in hot-rolled rod (footnote a) | — |
| 12 | elastic modulus | Table 4, Modulus of Elasticity, tension, GPa column; the imperial column prints 21.4 x 10^3 ksi for the same row | condition annealed (grade 1)temperature 871 C (1600 F)basis tension modulus, measured dynamically on 3/4 in hot-rolled rod (footnote a) | — |
| 13 | elastic modulus | Table 4, Modulus of Elasticity, tension, GPa column; the imperial column prints 21.5 x 10^3 ksi for the same row | condition solution-annealed (grade 2; Special Metals calls it solution-treated)temperature 871 C (1600 F)basis tension modulus, measured dynamically on 3/4 in hot-rolled rod (footnote a) | — |
| 14 | poissons ratio | Table 4, Poisson ratio column, annealed, printed for the 70 F row | condition annealed (grade 1)temperature 21 C (70 F) | — |
| 15 | poissons ratio | Table 4, Poisson ratio column, solution-treated, printed for the 70 F row | condition solution-annealed (grade 2; Special Metals calls it solution-treated)temperature 21 C (70 F) | — |
| 16 | ultimate tensile strength | Table 5, printed as 120-150 ksi (827-1034 MPa); the table footnote says these are composites and are not for specification | condition annealed (grade 1)product rod, bar and plate, composite for sizes up to 4 intemperature room temperature | — |
| 17 | yield strength | Table 5, printed as 60-95 ksi (414-655 MPa); composite values, not for specification | condition annealed (grade 1)product rod, bar and plate, composite for sizes up to 4 intemperature room temperature, 0.2 percent offset | — |
| 18 | elongation | Table 5 prints 60-30 percent; recorded here low to high | condition annealed (grade 1)product rod, bar and plate, composite for sizes up to 4 intemperature room temperature | — |
| 19 | ultimate tensile strength | Table 5, printed as 105-130 ksi (724-896 MPa); composite values, not for specification | condition solution-annealed (grade 2; Special Metals calls it solution-treated)product rod, bar and plate, composite for sizes up to 4 intemperature room temperature | — |
| 20 | yield strength | Table 5, printed as 42-60 ksi (290-414 MPa); composite values, not for specification | condition solution-annealed (grade 2; Special Metals calls it solution-treated)product rod, bar and plate, composite for sizes up to 4 intemperature room temperature, 0.2 percent offset | — |
| 21 | elongation | Table 5 prints 65-40 percent; recorded here low to high | condition solution-annealed (grade 2; Special Metals calls it solution-treated)product rod, bar and plate, composite for sizes up to 4 intemperature room temperature | — |
| 22 | ultimate tensile strength | Table 5, SHEET and STRIP, Annealed, printed as 120-150 ksi (827-1034 MPa); composite values, not for specification | condition annealed (grade 1)product sheet and strip, composite for sizes up to 4 intemperature room temperature | — |
| 23 | yield strength | Table 5, SHEET and STRIP, Annealed, printed as 60-90 ksi (414-621 MPa); composite values, not for specification | condition annealed (grade 1)product sheet and strip, composite for sizes up to 4 intemperature room temperature, 0.2 percent offset | — |
| 24 | ultimate tensile strength | Table 8, Effect of Annealing (1 Hour) on Room-Temperature Properties of Hot-Rolled Rod, 1800 F row | condition annealed (grade 1); 1 h anneal at 1800 F (982 C), inside the 1700-1900 F annealing rangeproduct hot-rolled rodtemperature room temperaturebasis annealing study, one hour at each temperature | — |
| 25 | yield strength | Table 8, same row, Yield Strength (0.2% offset) column | condition annealed (grade 1); 1 h anneal at 1800 F (982 C), inside the 1700-1900 F annealing rangeproduct hot-rolled rodtemperature room temperature, 0.2 percent offsetbasis annealing study, one hour at each temperature | — |
| 26 | ultimate tensile strength | Table 8, row 2100 F (1149 C), Tensile Strength column, printed as 116.0 ksi | condition solution-annealed (grade 2); 1 h anneal at 2100 F (1149 C), inside the 2000-2200 F solution treatment rangeproduct hot-rolled rodtemperature room temperaturebasis annealing study, one hour at each temperature | — |
| 27 | yield strength | Table 8, row 2100 F (1149 C), Yield Strength (0.2% offset) column, printed as 50.0 ksi | condition solution-annealed (grade 2); 1 h anneal at 2100 F (1149 C), inside the 2000-2200 F solution treatment rangeproduct hot-rolled rodtemperature room temperature, 0.2 percent offsetbasis annealing study, one hour at each temperature | — |
| 28 | ultimate tensile strength | Table 6, Effect of Intermediate-Temperature Exposure (2000 hrs), properties at exposure temperature, tensile strength, 1200 F row (1010.1 MPa) | condition annealed (grade 1), hot-rolled annealed barexposure 2000 hours at 1200 F (649 C) before testtemperature 1200 F (649 C), tested at the exposure temperature | — |
| 29 | yield strength | Table 6, same row, Properties at Exposure Temperature, Yield Strength (0.2% offset), printed as 106.5 ksi (734.3 MPa) | condition annealed (grade 1), hot-rolled annealed barexposure 2000 hours at 1200 F (649 C) before testtemperature 1200 F (649 C), tested at the exposure temperature, 0.2 percent offset | — |
| 30 | elongation | Table 6, No Exposure row, Properties at Room Temperature, Elongation | condition annealed (grade 1), hot-rolled annealed barexposure none (unexposed reference)temperature room temperature | — |
| 31 | elongation | Table 6, row 1200 (649), Properties at Room Temperature, Elongation | condition annealed (grade 1), hot-rolled annealed barexposure 2000 hours at 1200 F (649 C) before testtemperature room temperature, after exposure | — |
| 32 | fatigue strength | Fatigue Strength section, printed as 90,000 psi for smooth bar; the text names bar for a sheet test, and the value is kept as printed | condition annealed, cold-rolled annealed sheet (condition as printed)specimen smoothtest endurance limit at 10^8 cycles, completely reversed bending, room temperature | — |
| 33 | fatigue strength | Fatigue Strength section, printed as 35,000 psi for the notched specimen (Kt+3.3) | condition annealed, cold-rolled annealed sheet (condition as printed)specimen notched, Kt+3.3test endurance limit at 10^8 cycles, completely reversed bending, room temperature | — |
| 34 | Maximum service temperature | Introduction, printed as 1800 F (982 C) and recorded here in C | basis datasheet service range statement; the sentence says service from cryogenic to 1800 F (982 C) and is a range, not a specification limit | — |
| 35 | ultimate tensile strength | ATI product page, plate table, printed as 120 min ksi (827 min MPa) | condition annealed (grade 1)product plate (ASTM B443, ASME SB-443, AMS 5599)basis minimum as printed on the ATI product page | — |
| 36 | yield strength | ATI product page, plate table, printed as 60 min ksi (414 min MPa) | condition annealed (grade 1)product plate (ASTM B443, ASME SB-443, AMS 5599)basis minimum as printed on the ATI product page | — |
| 37 | elongation | ATI product page, plate table, printed as 30% min | condition annealed (grade 1)product plate (ASTM B443, ASME SB-443, AMS 5599)basis minimum as printed on the ATI product page | — |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Mild aqueous media: atmosphere, fresh and sea water, neutral salts and alkaline media | low | Almost no attack in mild environments (Special Metals).1 |
| Oxidising and non-oxidising chemicals, including hydrochloric and nitric acid wastes | low | Resists oxidising and non-oxidising chemicals, and was recommended for a storage tank for chemical wastes that include hydrochloric and nitric acid.2 |
| Chloride pitting and crevice attack | low | Very resistant to pitting and crevice corrosion because of its high molybdenum content (Special Metals; ATI).3 |
| Chloride-ion stress-corrosion cracking | none | Freedom from chloride-ion stress-corrosion cracking, credited to the high nickel content (Special Metals).4 |
| Sour oil and gas service (NACE MR0175) | not rated | Listed in NACE MR-01-75 (Special Metals); no sour-service test result was read.5 |
| Welding and heat-affected zones | low | Niobium stabilises the alloy against sensitisation, which prevents intergranular cracking after welding (Special Metals).6 |
| Air oxidation and scaling at high temperature | low | Excellent oxidation resistance up to 2,000 F (1,093 C) according to ATI; good scaling resistance in the Special Metals cyclic test at 1800 F.7 |
| Long exposure at intermediate temperatures near 1200 F | moderate | Hardens on exposure near 1200 F and loses ductility; no embrittling sigma phase was found after 1000 to 1800 F exposure (Special Metals).8 |
| Creep and rupture at high temperature under stress | not rated | The solution-annealed grade is recommended for the best creep and rupture resistance; the creep curves are graphs only.9 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Mild aqueous media: atmosphere, fresh and sea water, neutral salts and alkaline media | Special Metals says that in the atmosphere, fresh and sea water, neutral salts and alkaline media there is almost no attack. The statement is qualitative, and no exposure time or corrosion rate is printed. | basis qualitative statement, no exposure time or corrosion rate printed |
| 2 | Oxidising and non-oxidising chemicals, including hydrochloric and nitric acid wastes | Nickel and chromium give resistance to oxidising chemicals, and high nickel and molybdenum give resistance to non-oxidising environments. Special Metals notes that materials resisting one of these acids are normally severely attacked by the other. | basis qualitative statements, no concentration, temperature or exposure time printed |
| 3 | Chloride pitting and crevice attack | Special Metals says the high molybdenum content makes the alloy very resistant to pitting and crevice corrosion, and the ATI sheet says the same. The sources give no critical pitting temperature or ASTM G48 result. | basis qualitative statements, no test method printed |
| 4 | Chloride-ion stress-corrosion cracking | Special Metals says the high nickel content gives freedom from chloride-ion stress-corrosion cracking. The ATI sheet says the alloy shows good corrosion resistance to chloride ion stress corrosion cracking. | basis qualitative statements, no test stress or medium printed |
| 5 | Sour oil and gas service (NACE MR0175) | Special Metals says the alloy is listed in NACE MR-01-75, and the Wikipedia infobox gives NACE MR0175-3. No sour-service test data were read in this run. | standard NACE MR-01-75 (listed) |
| 6 | Welding and heat-affected zones | Special Metals says niobium acts to stabilise the alloy against sensitisation during welding, which prevents later intergranular cracking. The 625 welding products have a higher alloy content to offset segregation that can cause preferential weld corrosion. | basis qualitative statement, no weld test printed |
| 7 | Air oxidation and scaling at high temperature | ATI says the alloy shows excellent oxidation resistance up to 2,000 F (1,093 C). Special Metals says it has good resistance to oxidation and scaling at high temperature. Its cyclic scaling comparison at 1800 F is printed only as a graph, so no mass-loss number was read. | temperature up to 2000 F (1093 C), ATI; cyclic test at 1800 F, Special Metalstest cyclic weight-loss scaling test, shown as a graph (Figure 15 of the datasheet) |
| 8 | Long exposure at intermediate temperatures near 1200 F | Annealed rod exposed for 2000 hours at 1200 F gained room-temperature strength and lost ductility (Table 6). Special Metals says the hardening is sluggish precipitation of a niobium-rich gamma prime phase, which transforms to orthorhombic Ni3Nb on long heating. Its stability tests from 1000 to 1800 F showed no embrittling intermetallic phases such as sigma. | temperature 1200 F (649 C) for 2000 hours; stability tests 1000 to 1800 Ftest room-temperature tensile tests after exposure |
| 9 | Creep and rupture at high temperature under stress | Special Metals recommends the solution-treated condition for components that need optimum resistance to creep or rupture, and says annealed material is adequate for many creep uses. The creep and rupture curves (Figures 11 to 14) are graphs and were not read as numbers. | basis qualitative statement; graphical creep data not read |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
No GHS classification was read for the solid alloy. The hazard flags come from the PubChem nickel record (nickel is about 58 percent of this alloy) and from the Renishaw safety data sheet for the metal powder.
- Solid metal
- The PubChem aggregated nickel record lists skin sensitisation (H317, 99.9 percent of reports), suspected cancer (H351, 72.9 percent) and organ damage from prolonged exposure (H372, 99.7 percent).
- Powder and dust
- The Renishaw safety data sheet for the metal powder carries the signal word Danger and the codes H317, H334, H350, H360F and H372, and says the powder may form an explosible dust-air mixture.
If a part is held in the wrong temperature range
These results come from the datasheets and the Wikipedia summary of phase behaviour, not from field incidents.
- Long exposure near 1200 F
- After 2000 hours at 1200 F, room-temperature tensile strength rises from 140.0 to 176.0 ksi and elongation falls from 54 to 30 percent (Special Metals Table 6).
- Precipitates from 923 to 1148 K
- Wikipedia says precipitates form in the range 923 to 1148 K that are detrimental to creep properties, and that delta phase begins to form at 998 K.
Handling and heat treatment
- Forming
- Hot forming uses a furnace held at no more than 2150 F, with heavy forging from 2150 to 1850 F and lighter reductions down to 1700 F (Special Metals).
- Scale removal
- Heating scale is tightly adherent, so a fused-salt bath before pickling is usually recommended (Special Metals).
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Ageing and loss of ductility near 1200 Fmoderate severity | Long exposure, tested after 2000 hours at 1200 FRoom-temperature tensile strength rises from 140.0 ksi unexposed to 176.0 ksi after exposure, while elongation falls from 54 to 30 percent (Special Metals Table 6). |
| Precipitation that weakens creep resistancemoderate severity | Exposure in the range 923 to 1148 K; gamma double prime forms at 973 K and delta phase begins to form at 998 K (Wikipedia)Precipitates detrimental to creep properties form in that range. Wikipedia reports that rupture elongation is about half of the solution-treated value when they form, citing Mathew et al. |
| Notch sensitivity in fatiguehigh severity | A notched specimen, Kt+3.3, cut from cold-rolled annealed sheet, tested in completely reversed bending at room temperatureThe endurance limit at 10^8 cycles falls from 90,000 psi for a smooth specimen to 35,000 psi for the notched specimen. |
| Duplex grain structure in hot formingmoderate severity | Non-uniform reductions during hot formingA duplex grain structure can form. The datasheet asks for uniform reductions and final minimum reductions of 15 to 20 percent for open-die work. |
Handling and storage
- Anneal hot- or cold-formed parts at 1700 to 1900 F for times set by thickness, and solution treat at 2000 to 2200 F (Special Metals). ATI gives 1600 to 1900 F for the anneal (ATI TDS).
- Remove sulphur-bearing lubricants before heat treating and pickling (ATI TDS).
- Use a fused-salt bath before pickling to remove the oxide that heating forms (Special Metals).
- Hot form in a furnace held at no more than 2150 F, with heavy forging from 2150 to 1850 F and lighter reductions down to 1700 F. Use uniform reductions to guard against duplex grain (Special Metals).
- Stress-relieve cold-drawn material at 1100 to 1400 F; stress relief is virtually complete at 1600 F (Special Metals).
- For welds, use INCONEL Filler Metal 625 (gas-tungsten-arc) or Welding Electrode 112 (shielded-metal-arc). The datasheet says the weld metal needs no postweld heat treatment to keep its strength and ductility (Special Metals).
Mitigations
- Above 1200 F, specify the solution-treated (solution-annealed, grade 2) condition where creep or rupture resistance is critical. At 1200 F and below, the datasheet recommends hot-finished, cold-finished or annealed conditions (Special Metals).
- Heating to 1148 K for 5 hours dissolves the gamma double prime and delta precipitates back into the matrix, which recovers creep properties (Wikipedia).
- Control powder dust: do not breathe dust (P260), and wear respiratory protection where ventilation is inadequate (P284) (Renishaw SDS, powder).
- Use the matching over-alloyed filler metals for welds. The 625 welding products offset segregation that can cause preferential weld corrosion (Special Metals).
Supply and geography
How common the raw materials are and where they come from.
Nickel
Globally, nickel resources have been estimated to contain more than 350 million tons of nickel (USGS)
- Top producers (2025)
- Indonesia 66.7%, Philippines 6.9%, Russia 5.1%, Canada 3.6%
- Recycling
- In 2025, nickel recovered from scrap accounted for approximately 60% of apparent consumption (USGS).
- Substitutes
- Low-nickel, duplex, or ultrahigh-chromium stainless steels have been substituted for austenitic grades in construction. Titanium alloys can substitute for nickel or nickel-base alloys in corrosive environments (USGS).
Chromium
World resources are greater than 12 billion tons of shipping-grade chromite (USGS)
- Top producers (2025)
- South Africa 45.1%, Turkey 17.6%, Kazakhstan 13.7%, India 5.9%
- Recycling
- In 2025, recycled chromium in reported stainless-steel scrap receipts accounted for 21% of apparent consumption (USGS).
- Substitutes
- Chromium has no substitute in stainless steel, the leading end use, or in superalloys, the major strategic end use (USGS).
Molybdenum
Identified resources in the United States are about 5.4 million tons and, in the rest of the world, about 20 million tons (USGS)
- Top producers (2025)
- China 37.3%, Chile 16.2%, United States 15.4%, Peru 15%, Mexico 6.5%
- Recycling
- Molybdenum is recycled as a component of catalysts, ferrous scrap and superalloy scrap; the recycled amount may be as much as 30% of apparent supply (USGS).
- Substitutes
- There is little substitution for molybdenum in steels and cast irons. Potential substitutes in alloy steels include boron, chromium, niobium and vanadium (USGS).
Niobium
World resources of niobium are more than adequate to supply projected needs (USGS)
- Top producers (2025)
- Brazil 92.9%, Canada 5.4%
- Recycling
- Niobium scrap recovery was negligible; recycled niobium may have been as much as 20% of apparent consumption (USGS).
- Substitutes
- Ceramic matrix composites, molybdenum, tantalum and tungsten can replace niobium in high-temperature superalloy applications, with a performance loss or higher cost (USGS).
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: inconel-625
spore_version: 0.2
family: nickel-alloys
name: Inconel 625
abbreviation: IN625 (UNS N06625)
role: corrosion-resistant solid-solution nickel superalloy
category: metals
type: nickel-superalloys
summary: |
Inconel 625 (UNS N06625, W.Nr. 2.4856) is a nickel-chromium-molybdenum-niobium alloy. Its strength comes from solid solution, so it needs no precipitation-hardening treatment. Special Metals gives a melting range of 1290 to 1350 C and a yield strength of 60 to 95 ksi for the annealed (grade 1) condition, which is stronger than the solution-annealed (grade 2) condition. It is used for corrosion-resistant chemical plant and marine parts, and for aerospace ducting and rocket tubing.
best_for: Corrosion-resistant parts that also need strength and good weldability, such as chemical plant, marine hardware, aerospace ducting and rocket tubing
weakest_at: Long exposure near 1200 F hardens the annealed alloy and cuts its room-temperature elongation from 54 to 30 percent after 2000 hours
identity:
formula: 'Nickel-chromium-molybdenum-niobium solid-solution alloy: 58.0 min Ni, 20.0 to 23.0 Cr, 8.0 to 10.0 Mo, 3.15 to 4.15 Nb plus Ta, 5.0 max Fe, 1.0 max Co (if determined), 0.50 max Mn, 0.50 max Si, 0.40 max Al, 0.40 max Ti, 0.10 max C, 0.015 max P, 0.015 max S (wt%)'
source: sm625
where: Table 1, Limiting Chemical Composition, % (Special Metals datasheet); UNS N06625 and W.Nr. 2.4856 from the introduction and the Available Products section
designations:
- system: UNS
code: N06625
source: sm625
where: Introduction, and Available Products and Specifications (designated as UNS N06625)
- system: EN
code: '2.4856'
source: sm625
where: Available Products and Specifications; the Wikipedia infobox also gives EN 2.4856
- system: ISO
code: NW6625
source: sm625
where: Available Products and Specifications
- system: ASTM
code: B 443
source: sm625
where: Available Products and Specifications, plate, sheet and strip
- system: ASTM
code: B 444
note: B 829; ASME SB 444, SB 829
source: sm625
where: Available Products and Specifications, pipe and tube
- system: ASTM
code: B 446
source: sm625
where: Available Products and Specifications, rod, bar, wire and forging stock
- system: AMS
code: '5599'
source: ati-tds
where: 'ATI TDS, Specifications: AMS 5599 with ASTM B 443 (sheet, strip, plate); AMS 5666 (bars, forgings, extrusions, rings); AMS 5837 (welding wire)'
- system: AMS
code: '5666'
source: ati-tds
where: 'ATI TDS, Specifications: AMS 5599 with ASTM B 443 (sheet, strip, plate); AMS 5666 (bars, forgings, extrusions, rings); AMS 5837 (welding wire)'
- system: AMS
code: '5837'
source: ati-tds
where: 'ATI TDS, Specifications: AMS 5599 with ASTM B 443 (sheet, strip, plate); AMS 5666 (bars, forgings, extrusions, rings); AMS 5837 (welding wire)'
- system: MIL
code: N-24687
source: ati-tds
where: 'ATI TDS, Specifications: bars, forgings, extrusions and rings'
- system: MIL
code: MIL-DTL-24799
source: ati-tds
where: 'ATI TDS, Specifications: bars, forgings, extrusions and rings'
- system: EN
code: '10095'
source: sm625
where: 'Available Products and Specifications: rod, bar and sections; plate, sheet and strip'
- system: NACE
code: MR-01-75
source: sm625
where: 'Available Products and Specifications: listed in NACE MR-01-75; the Wikipedia infobox gives NACE MR0175-3'
- system: Trade name
code: INCONEL alloy 625
source: sm625
where: Datasheet title (Special Metals trademark)
- system: Trade name
code: ATI 625
source: ati-page
where: ATI product page, ATI 625 Nickel-Based Alloy
- system: Trade name
code: Haynes 625
source: wiki625
where: Introduction, other well known names
- system: Trade name
code: Nickelvac 625
source: wiki625
where: Introduction, other well known names
- system: Trade name
code: Nicrofer 6020
source: wiki625
where: Introduction, other well known names
- system: Trade name
code: Altemp 625
source: wiki625
where: Introduction, other well known names
- system: Trade name
code: Chronin 625
source: wiki625
where: Introduction, other well known names
tags:
environments:
- launch
stresses: []
applications:
- propulsion-and-tanks
- structures
- thermal-control
properties:
- benchmark: density
value: 8.44
unit: g/cm3
scope: material
conditions:
basis: datasheet physical constant, no test temperature printed
unit_in_source: gram/cc (0.305 lb/cu in printed alongside)
method: Table 2, Physical Constants, Density, printed as 0.305 lb/cu in and 8.44 gram/cc; the gram/cc value is kept
status: ground
source: sm625
where: Table 2, Density, gram/cc row
- benchmark: melting_point
value: 1290
value_high: 1350
bound: range
unit: °C
scope: material
conditions:
basis: melting range as printed in Table 2 (2350 to 2460 F)
method: Table 2, metric row printed as 1290-1350 C; the ATI TDS prints 1,288 to 1,343 C (2,350 to 2,450 F), and the Special Metals range is kept here
status: ground
source: sm625
where: Table 2, Melting Range, C row
- benchmark: specific_heat
value: 410
unit: J/(kg·K)
scope: material
conditions:
basis: at 70 F (21 C); printed as 0.098 Btu/lb F
unit_in_source: J/kg °C
method: Table 2, metric value in parentheses; the datasheet marks the row as calculated (footnote a)
status: calculated
source: sm625
where: Table 2, Specific Heat, 70 F (21 C) row
- benchmark: curie_temperature
value: -196
bound: upper
unit: °C
scope: material
conditions:
basis: printed as less than -320 F; metric value -196 C
method: Table 2, Curie Temperature, C row; the metric row has no less-than sign, so the value is recorded as an upper bound
status: ground
source: sm625
where: Table 2, Curie Temperature, C row
- benchmark: thermal_conductivity
value: 9.8
unit: W/m°C
scope: material
conditions:
basis: at 21 C (70 F); material annealed 2100 F for 1 h (footnote c); measured at Battelle (footnote b)
method: Table 3, Thermal Conductivity, metric column; the same row prints 68 Btu·in/ft²·h·°F at 70 F
status: ground
source: sm625
where: Table 3, Thermal Conductivity, row 21 C (70 F)
- benchmark: thermal_conductivity
value: 25.2
unit: W/m°C
scope: material
conditions:
basis: at 982 C (1800 F); material annealed 2100 F for 1 h (footnote c)
method: Table 3, Thermal Conductivity, metric column, row 982 C (1800 F)
status: ground
source: sm625
where: Table 3, Thermal Conductivity, row 982 C (1800 F)
- benchmark: electrical_resistivity
value: 129
unit: µΩ-cm
scope: material
conditions:
basis: at 21 C (70 F); material annealed 2100 F for 1 h (footnote c)
method: Table 3, Electrical Resistivity, metric column; the imperial column prints 776 ohm circ mil/ft at 70 F
status: ground
source: sm625
where: Table 3, Electrical Resistivity, row 21 C (70 F)
- benchmark: cte
value: 12.8
unit: ppm/°C
scope: material
conditions:
basis: mean linear expansion from 21 C (70 F) to 93 C (200 F), footnote a
material: not stated in the datasheet
unit_in_source: µm/µm·°C
method: Table 3, Mean Linear Expansion, metric column (µm/µm·°C is the same unit as ppm/°C); the imperial column prints 7.1 x 10^-6 in/in·°F at 200 F
status: ground
source: sm625
where: Table 3, Mean Linear Expansion, row 93 C (200 F)
- benchmark: cte
value: 14.8
unit: ppm/°C
scope: material
conditions:
basis: mean linear expansion from 21 C (70 F) to 649 C (1200 F), footnote a
material: not stated in the datasheet
unit_in_source: µm/µm·°C
method: Table 3, Mean Linear Expansion, metric column, row 649 C; the imperial column prints 8.2 x 10^-6 in/in·°F at 1200 F
status: ground
source: sm625
where: Table 3, Mean Linear Expansion, row 649 C (1200 F)
- benchmark: elastic_modulus
value: 207.5
unit: GPa
scope: material
conditions:
condition: annealed (grade 1)
temperature: 21 C (70 F)
basis: tension modulus, measured dynamically on 3/4 in hot-rolled rod (footnote a)
method: Table 4, Modulus of Elasticity, tension, GPa column; the imperial column prints 30.1 x 10^3 ksi for the same row
status: ground
source: sm625
where: Table 4, Modulus of Elasticity, row 70 F (21 C), Annealed column
- benchmark: elastic_modulus
value: 204.8
unit: GPa
scope: material
conditions:
condition: solution-annealed (grade 2; Special Metals calls it solution-treated)
temperature: 21 C (70 F)
basis: tension modulus, measured dynamically on 3/4 in hot-rolled rod (footnote a)
method: Table 4, Modulus of Elasticity, tension, GPa column; the imperial column prints 29.7 x 10^3 ksi for the same row
status: ground
source: sm625
where: Table 4, Modulus of Elasticity, row 70 F (21 C), Solution-Treated column
- benchmark: elastic_modulus
value: 147.5
unit: GPa
scope: material
conditions:
condition: annealed (grade 1)
temperature: 871 C (1600 F)
basis: tension modulus, measured dynamically on 3/4 in hot-rolled rod (footnote a)
method: Table 4, Modulus of Elasticity, tension, GPa column; the imperial column prints 21.4 x 10^3 ksi for the same row
status: ground
source: sm625
where: Table 4, Modulus of Elasticity, row 1600 F (871 C), Annealed column
- benchmark: elastic_modulus
value: 148.2
unit: GPa
scope: material
conditions:
condition: solution-annealed (grade 2; Special Metals calls it solution-treated)
temperature: 871 C (1600 F)
basis: tension modulus, measured dynamically on 3/4 in hot-rolled rod (footnote a)
method: Table 4, Modulus of Elasticity, tension, GPa column; the imperial column prints 21.5 x 10^3 ksi for the same row
status: ground
source: sm625
where: Table 4, Modulus of Elasticity, row 1600 F (871 C), Solution-Treated column
- benchmark: poissons_ratio
value: 0.278
unit: '-'
scope: material
conditions:
condition: annealed (grade 1)
temperature: 21 C (70 F)
method: Table 4, Poisson ratio column, annealed, printed for the 70 F row
status: ground
source: sm625
where: Table 4, Poisson ratio, row 70 F (21 C), Annealed column
- benchmark: poissons_ratio
value: 0.312
unit: '-'
scope: material
conditions:
condition: solution-annealed (grade 2; Special Metals calls it solution-treated)
temperature: 21 C (70 F)
method: Table 4, Poisson ratio column, solution-treated, printed for the 70 F row
status: ground
source: sm625
where: Table 4, Poisson ratio, row 70 F (21 C), Solution-Treated column
- benchmark: ultimate_tensile_strength
value: 120
value_high: 150
bound: range
unit: ksi
scope: material
conditions:
condition: annealed (grade 1)
product: rod, bar and plate, composite for sizes up to 4 in
temperature: room temperature
method: Table 5, printed as 120-150 ksi (827-1034 MPa); the table footnote says these are composites and are not for specification
status: ground
source: sm625
where: Table 5, Nominal Room-Temperature Mechanical Properties, ROD BAR PLATE, Annealed row, Tensile Strength
- benchmark: yield_strength
value: 60
value_high: 95
bound: range
unit: ksi
scope: material
conditions:
condition: annealed (grade 1)
product: rod, bar and plate, composite for sizes up to 4 in
temperature: room temperature, 0.2 percent offset
method: Table 5, printed as 60-95 ksi (414-655 MPa); composite values, not for specification
status: ground
source: sm625
where: Table 5, ROD BAR PLATE, Annealed row, Yield Strength (0.2% Offset)
- benchmark: elongation
value: 30
value_high: 60
bound: range
unit: '%'
scope: material
conditions:
condition: annealed (grade 1)
product: rod, bar and plate, composite for sizes up to 4 in
temperature: room temperature
method: Table 5 prints 60-30 percent; recorded here low to high
status: ground
source: sm625
where: Table 5, ROD BAR PLATE, Annealed row, Elongation
- benchmark: ultimate_tensile_strength
value: 105
value_high: 130
bound: range
unit: ksi
scope: material
conditions:
condition: solution-annealed (grade 2; Special Metals calls it solution-treated)
product: rod, bar and plate, composite for sizes up to 4 in
temperature: room temperature
method: Table 5, printed as 105-130 ksi (724-896 MPa); composite values, not for specification
status: ground
source: sm625
where: Table 5, ROD BAR PLATE, Solution-Treated row, Tensile Strength
- benchmark: yield_strength
value: 42
value_high: 60
bound: range
unit: ksi
scope: material
conditions:
condition: solution-annealed (grade 2; Special Metals calls it solution-treated)
product: rod, bar and plate, composite for sizes up to 4 in
temperature: room temperature, 0.2 percent offset
method: Table 5, printed as 42-60 ksi (290-414 MPa); composite values, not for specification
status: ground
source: sm625
where: Table 5, ROD BAR PLATE, Solution-Treated row, Yield Strength (0.2% Offset)
- benchmark: elongation
value: 40
value_high: 65
bound: range
unit: '%'
scope: material
conditions:
condition: solution-annealed (grade 2; Special Metals calls it solution-treated)
product: rod, bar and plate, composite for sizes up to 4 in
temperature: room temperature
method: Table 5 prints 65-40 percent; recorded here low to high
status: ground
source: sm625
where: Table 5, ROD BAR PLATE, Solution-Treated row, Elongation
- benchmark: ultimate_tensile_strength
value: 120
value_high: 150
bound: range
unit: ksi
scope: material
conditions:
condition: annealed (grade 1)
product: sheet and strip, composite for sizes up to 4 in
temperature: room temperature
method: Table 5, SHEET and STRIP, Annealed, printed as 120-150 ksi (827-1034 MPa); composite values, not for specification
status: ground
source: sm625
where: Table 5, SHEET and STRIP, Annealed row, Tensile Strength
- benchmark: yield_strength
value: 60
value_high: 90
bound: range
unit: ksi
scope: material
conditions:
condition: annealed (grade 1)
product: sheet and strip, composite for sizes up to 4 in
temperature: room temperature, 0.2 percent offset
method: Table 5, SHEET and STRIP, Annealed, printed as 60-90 ksi (414-621 MPa); composite values, not for specification
status: ground
source: sm625
where: Table 5, SHEET and STRIP, Annealed row, Yield Strength (0.2% Offset)
- benchmark: ultimate_tensile_strength
value: 143.5
unit: ksi
scope: material
conditions:
condition: annealed (grade 1); 1 h anneal at 1800 F (982 C), inside the 1700-1900 F annealing range
product: hot-rolled rod
temperature: room temperature
basis: annealing study, one hour at each temperature
method: Table 8, Effect of Annealing (1 Hour) on Room-Temperature Properties of Hot-Rolled Rod, 1800 F row
status: ground
source: sm625
where: Table 8, row 1800 F (982 C), Tensile Strength column
- benchmark: yield_strength
value: 83.6
unit: ksi
scope: material
conditions:
condition: annealed (grade 1); 1 h anneal at 1800 F (982 C), inside the 1700-1900 F annealing range
product: hot-rolled rod
temperature: room temperature, 0.2 percent offset
basis: annealing study, one hour at each temperature
method: Table 8, same row, Yield Strength (0.2% offset) column
status: ground
source: sm625
where: Table 8, row 1800 F (982 C), Yield Strength column
- benchmark: ultimate_tensile_strength
value: 116
unit: ksi
scope: material
conditions:
condition: solution-annealed (grade 2); 1 h anneal at 2100 F (1149 C), inside the 2000-2200 F solution treatment range
product: hot-rolled rod
temperature: room temperature
basis: annealing study, one hour at each temperature
method: Table 8, row 2100 F (1149 C), Tensile Strength column, printed as 116.0 ksi
status: ground
source: sm625
where: Table 8, row 2100 F (1149 C), Tensile Strength column
- benchmark: yield_strength
value: 50
unit: ksi
scope: material
conditions:
condition: solution-annealed (grade 2); 1 h anneal at 2100 F (1149 C), inside the 2000-2200 F solution treatment range
product: hot-rolled rod
temperature: room temperature, 0.2 percent offset
basis: annealing study, one hour at each temperature
method: Table 8, row 2100 F (1149 C), Yield Strength (0.2% offset) column, printed as 50.0 ksi
status: ground
source: sm625
where: Table 8, row 2100 F (1149 C), Yield Strength column
- benchmark: ultimate_tensile_strength
value: 146.5
unit: ksi
scope: material
conditions:
condition: annealed (grade 1), hot-rolled annealed bar
exposure: 2000 hours at 1200 F (649 C) before test
temperature: 1200 F (649 C), tested at the exposure temperature
method: Table 6, Effect of Intermediate-Temperature Exposure (2000 hrs), properties at exposure temperature, tensile strength, 1200 F row (1010.1 MPa)
status: ground
source: sm625
where: Table 6, row 1200 (649), Properties at Exposure Temperature, Tensile Strength
- benchmark: yield_strength
value: 106.5
unit: ksi
scope: material
conditions:
condition: annealed (grade 1), hot-rolled annealed bar
exposure: 2000 hours at 1200 F (649 C) before test
temperature: 1200 F (649 C), tested at the exposure temperature, 0.2 percent offset
method: Table 6, same row, Properties at Exposure Temperature, Yield Strength (0.2% offset), printed as 106.5 ksi (734.3 MPa)
status: ground
source: sm625
where: Table 6, row 1200 (649), Properties at Exposure Temperature, Yield Strength
- benchmark: elongation
value: 54
unit: '%'
scope: material
conditions:
condition: annealed (grade 1), hot-rolled annealed bar
exposure: none (unexposed reference)
temperature: room temperature
method: Table 6, No Exposure row, Properties at Room Temperature, Elongation
status: ground
source: sm625
where: Table 6, No Exposure row, Properties at Room Temperature, Elongation
- benchmark: elongation
value: 30
unit: '%'
scope: material
conditions:
condition: annealed (grade 1), hot-rolled annealed bar
exposure: 2000 hours at 1200 F (649 C) before test
temperature: room temperature, after exposure
method: Table 6, row 1200 (649), Properties at Room Temperature, Elongation
status: ground
source: sm625
where: Table 6, row 1200 (649), Properties at Room Temperature, Elongation
- benchmark: fatigue_strength
value: 90000
unit: psi
scope: material
conditions:
condition: annealed, cold-rolled annealed sheet (condition as printed)
specimen: smooth
test: endurance limit at 10^8 cycles, completely reversed bending, room temperature
method: Fatigue Strength section, printed as 90,000 psi for smooth bar; the text names bar for a sheet test, and the value is kept as printed
status: ground
source: sm625
where: Fatigue Strength section, first paragraph
- benchmark: fatigue_strength
value: 35000
unit: psi
scope: material
conditions:
condition: annealed, cold-rolled annealed sheet (condition as printed)
specimen: notched, Kt+3.3
test: endurance limit at 10^8 cycles, completely reversed bending, room temperature
method: Fatigue Strength section, printed as 35,000 psi for the notched specimen (Kt+3.3)
status: ground
source: sm625
where: Fatigue Strength section, first paragraph
- benchmark: max_service_temp
value: 982
unit: °C
scope: material
conditions:
basis: datasheet service range statement; the sentence says service from cryogenic to 1800 F (982 C) and is a range, not a specification limit
method: Introduction, printed as 1800 F (982 C) and recorded here in C
status: ground
source: sm625
where: Introduction, first paragraph
- benchmark: ultimate_tensile_strength
value: 120
bound: lower
unit: ksi
scope: material
conditions:
condition: annealed (grade 1)
product: plate (ASTM B443, ASME SB-443, AMS 5599)
basis: minimum as printed on the ATI product page
method: ATI product page, plate table, printed as 120 min ksi (827 min MPa)
status: ground
source: ati-page
where: ATI product page, Plate table, annealed (Grade 1) condition, Tensile Strength
- benchmark: yield_strength
value: 60
bound: lower
unit: ksi
scope: material
conditions:
condition: annealed (grade 1)
product: plate (ASTM B443, ASME SB-443, AMS 5599)
basis: minimum as printed on the ATI product page
method: ATI product page, plate table, printed as 60 min ksi (414 min MPa)
status: ground
source: ati-page
where: ATI product page, Plate table, annealed (Grade 1) condition, Yield Strength
- benchmark: elongation
value: 30
bound: lower
unit: '%'
scope: material
conditions:
condition: annealed (grade 1)
product: plate (ASTM B443, ASME SB-443, AMS 5599)
basis: minimum as printed on the ATI product page
method: ATI product page, plate table, printed as 30% min
status: ground
source: ati-page
where: ATI product page, Plate table, annealed (Grade 1) condition, Elongation
corrosion:
- environment: 'Mild aqueous media: atmosphere, fresh and sea water, neutral salts and alkaline media'
headline: Almost no attack in mild environments (Special Metals).
effect: Special Metals says that in the atmosphere, fresh and sea water, neutral salts and alkaline media there is almost no attack. The statement is qualitative, and no exposure time or corrosion rate is printed.
rating: low
conditions:
basis: qualitative statement, no exposure time or corrosion rate printed
source: sm625
where: Corrosion Resistance, Aqueous Corrosion, first paragraph
- environment: Oxidising and non-oxidising chemicals, including hydrochloric and nitric acid wastes
headline: Resists oxidising and non-oxidising chemicals, and was recommended for a storage tank for chemical wastes that include hydrochloric and nitric acid.
effect: Nickel and chromium give resistance to oxidising chemicals, and high nickel and molybdenum give resistance to non-oxidising environments. Special Metals notes that materials resisting one of these acids are normally severely attacked by the other.
rating: low
conditions:
basis: qualitative statements, no concentration, temperature or exposure time printed
source: sm625
where: Corrosion Resistance, Aqueous Corrosion, first two paragraphs
- environment: Chloride pitting and crevice attack
headline: Very resistant to pitting and crevice corrosion because of its high molybdenum content (Special Metals; ATI).
effect: Special Metals says the high molybdenum content makes the alloy very resistant to pitting and crevice corrosion, and the ATI sheet says the same. The sources give no critical pitting temperature or ASTM G48 result.
rating: low
conditions:
basis: qualitative statements, no test method printed
source: sm625
where: Corrosion Resistance, Aqueous Corrosion, first paragraph
- environment: Chloride-ion stress-corrosion cracking
headline: Freedom from chloride-ion stress-corrosion cracking, credited to the high nickel content (Special Metals).
effect: Special Metals says the high nickel content gives freedom from chloride-ion stress-corrosion cracking. The ATI sheet says the alloy shows good corrosion resistance to chloride ion stress corrosion cracking.
rating: none
conditions:
basis: qualitative statements, no test stress or medium printed
source: sm625
where: Corrosion Resistance, Aqueous Corrosion, first paragraph
- environment: Sour oil and gas service (NACE MR0175)
headline: Listed in NACE MR-01-75 (Special Metals); no sour-service test result was read.
effect: Special Metals says the alloy is listed in NACE MR-01-75, and the Wikipedia infobox gives NACE MR0175-3. No sour-service test data were read in this run.
rating: unknown
conditions:
standard: NACE MR-01-75 (listed)
source: sm625
where: Available Products and Specifications
- environment: Welding and heat-affected zones
headline: Niobium stabilises the alloy against sensitisation, which prevents intergranular cracking after welding (Special Metals).
effect: Special Metals says niobium acts to stabilise the alloy against sensitisation during welding, which prevents later intergranular cracking. The 625 welding products have a higher alloy content to offset segregation that can cause preferential weld corrosion.
rating: low
conditions:
basis: qualitative statement, no weld test printed
source: sm625
where: Corrosion Resistance, Aqueous Corrosion, first paragraph; Welding section
- environment: Air oxidation and scaling at high temperature
headline: Excellent oxidation resistance up to 2,000 F (1,093 C) according to ATI; good scaling resistance in the Special Metals cyclic test at 1800 F.
effect: ATI says the alloy shows excellent oxidation resistance up to 2,000 F (1,093 C). Special Metals says it has good resistance to oxidation and scaling at high temperature. Its cyclic scaling comparison at 1800 F is printed only as a graph, so no mass-loss number was read.
rating: low
conditions:
temperature: up to 2000 F (1093 C), ATI; cyclic test at 1800 F, Special Metals
test: cyclic weight-loss scaling test, shown as a graph (Figure 15 of the datasheet)
source: ati-tds
where: Oxidation Resistance, page 1 of the ATI TDS
- environment: Long exposure at intermediate temperatures near 1200 F
headline: Hardens on exposure near 1200 F and loses ductility; no embrittling sigma phase was found after 1000 to 1800 F exposure (Special Metals).
effect: Annealed rod exposed for 2000 hours at 1200 F gained room-temperature strength and lost ductility (Table 6). Special Metals says the hardening is sluggish precipitation of a niobium-rich gamma prime phase, which transforms to orthorhombic Ni3Nb on long heating. Its stability tests from 1000 to 1800 F showed no embrittling intermetallic phases such as sigma.
rating: moderate
conditions:
temperature: 1200 F (649 C) for 2000 hours; stability tests 1000 to 1800 F
test: room-temperature tensile tests after exposure
source: sm625
where: Mechanical Properties, Table 6; Microstructure section
- environment: Creep and rupture at high temperature under stress
headline: The solution-annealed grade is recommended for the best creep and rupture resistance; the creep curves are graphs only.
effect: Special Metals recommends the solution-treated condition for components that need optimum resistance to creep or rupture, and says annealed material is adequate for many creep uses. The creep and rupture curves (Figures 11 to 14) are graphs and were not read as numbers.
rating: unknown
conditions:
basis: qualitative statement; graphical creep data not read
source: sm625
where: Creep and Rupture Strength section; Mechanical Properties section
risks:
hazards:
- text: 'PubChem aggregated GHS for nickel metal, from 4778 company reports and 86 ECHA C&L notifications: H317 in 99.9% of the reports that give a code, H351 in 72.9%, H372 in 99.7%, H350 in 22.5%, H360F in 18%, H341 in 13.5%, H334 in 10.3% and H412 in 47.2%. The record is for nickel, which is about 58 percent of this alloy, not for the alloy itself.'
ghs:
- H317
- H351
- H372
- H350
- H360F
- H341
- H334
- H412
source: pubchem-nickel
where: Safety and Hazards, GHS Classification (PubChem PUG View JSON, aggregated ECHA C&L notifications)
- text: 'Renishaw safety data sheet for Inconel 625 metal powder (document H-5800-3483-02-A_EN, SDS date 1/27/2023, version 1.0): classified Skin Sens. 1, Resp. Sens. 1, Carc. 1B, Repr. 1B and STOT RE 1, with signal word Danger. This applies to the powder for additive manufacture, not to solid stock.'
ghs:
- H317
- H334
- H350
- H360F
- H372
source: renishaw-sds
where: Sections 1 and 2 (identification, hazard classification and label elements)
- text: The powder SDS says it may form an explosible dust-air mixture when dispersed, and that dust deposits should not be allowed to accumulate because they may form an explosive mixture.
ghs: []
source: renishaw-sds
where: Section 2 (other hazards); Section 6 (accidental release measures)
failure_risks:
- mode: Ageing and loss of ductility near 1200 F
trigger: Long exposure, tested after 2000 hours at 1200 F
consequence: Room-temperature tensile strength rises from 140.0 ksi unexposed to 176.0 ksi after exposure, while elongation falls from 54 to 30 percent (Special Metals Table 6).
severity: moderate
source: sm625
where: Mechanical Properties, Table 6
- mode: Precipitation that weakens creep resistance
trigger: Exposure in the range 923 to 1148 K; gamma double prime forms at 973 K and delta phase begins to form at 998 K (Wikipedia)
consequence: Precipitates detrimental to creep properties form in that range. Wikipedia reports that rupture elongation is about half of the solution-treated value when they form, citing Mathew et al.
severity: moderate
source: wiki625
where: Creep and microstructure sections (Wikipedia Inconel 625)
- mode: Notch sensitivity in fatigue
trigger: A notched specimen, Kt+3.3, cut from cold-rolled annealed sheet, tested in completely reversed bending at room temperature
consequence: The endurance limit at 10^8 cycles falls from 90,000 psi for a smooth specimen to 35,000 psi for the notched specimen.
severity: high
source: sm625
where: Fatigue Strength section
- mode: Duplex grain structure in hot forming
trigger: Non-uniform reductions during hot forming
consequence: A duplex grain structure can form. The datasheet asks for uniform reductions and final minimum reductions of 15 to 20 percent for open-die work.
severity: moderate
source: sm625
where: Hot and cold forming section
side_effects: []
handling:
- text: Anneal hot- or cold-formed parts at 1700 to 1900 F for times set by thickness, and solution treat at 2000 to 2200 F (Special Metals). ATI gives 1600 to 1900 F for the anneal (ATI TDS).
source: sm625
where: Working Instructions, Heating
- text: Remove sulphur-bearing lubricants before heat treating and pickling (ATI TDS).
source: ati-tds
where: Special Precautions
- text: Use a fused-salt bath before pickling to remove the oxide that heating forms (Special Metals).
source: sm625
where: Pickling
- text: Hot form in a furnace held at no more than 2150 F, with heavy forging from 2150 to 1850 F and lighter reductions down to 1700 F. Use uniform reductions to guard against duplex grain (Special Metals).
source: sm625
where: Hot and cold forming
- text: Stress-relieve cold-drawn material at 1100 to 1400 F; stress relief is virtually complete at 1600 F (Special Metals).
source: sm625
where: Working Instructions, Heating (stress relief); Tables 8 and 9
- text: For welds, use INCONEL Filler Metal 625 (gas-tungsten-arc) or Welding Electrode 112 (shielded-metal-arc). The datasheet says the weld metal needs no postweld heat treatment to keep its strength and ductility (Special Metals).
source: sm625
where: Welding section
mitigations:
- text: Above 1200 F, specify the solution-treated (solution-annealed, grade 2) condition where creep or rupture resistance is critical. At 1200 F and below, the datasheet recommends hot-finished, cold-finished or annealed conditions (Special Metals).
source: sm625
where: Mechanical Properties, service recommendations
- text: Heating to 1148 K for 5 hours dissolves the gamma double prime and delta precipitates back into the matrix, which recovers creep properties (Wikipedia).
source: wiki625
where: Microstructure section (Wikipedia Inconel 625)
- text: 'Control powder dust: do not breathe dust (P260), and wear respiratory protection where ventilation is inadequate (P284) (Renishaw SDS, powder).'
source: renishaw-sds
where: Section 2, precautionary statements
- text: Use the matching over-alloyed filler metals for welds. The 625 welding products offset segregation that can cause preferential weld corrosion (Special Metals).
source: sm625
where: Welding section; All-Weld-Metal Properties
uses:
- application: propulsion-and-tanks
device: Thrust-chamber tubing for rocket engines, fuel and hydraulic line tubing, and engine exhaust systems
example: Special Metals lists thrust-chamber tubing for rocket engines, fuel and hydraulic line tubing, engine exhaust systems and combustion-system transition liners among its aerospace uses.
source: sm625
where: Introduction, aerospace paragraph
- application: structures
device: Aircraft ducting systems, resistance-welded honeycomb structures housing engine controls, and turbine shroud rings
example: Special Metals names these aerospace uses. The ATI TDS says the alloy is widely used in aerospace for airframe and jet engine applications.
source: sm625
where: Introduction, aerospace paragraph; ATI TDS, Introduction
- application: thermal-control
device: Heat-exchanger tubing in environmental control systems
example: Special Metals lists heat-exchanger tubing in environmental control systems among its aerospace uses.
source: sm625
where: Introduction, aerospace paragraph
supply:
- subject: Nickel
abundance: Globally, nickel resources have been estimated to contain more than 350 million tons of nickel (USGS)
producers:
- country: Indonesia
share_percent: 66.7
year: 2025
- country: Philippines
share_percent: 6.9
year: 2025
- country: Russia
share_percent: 5.1
year: 2025
- country: Canada
share_percent: 3.6
year: 2025
recycling: In 2025, nickel recovered from scrap accounted for approximately 60% of apparent consumption (USGS).
substitutes:
- Low-nickel, duplex, or ultrahigh-chromium stainless steels have been substituted for austenitic grades in construction. Titanium alloys can substitute for nickel or nickel-base alloys in corrosive environments (USGS).
source: usgs-mcs2026-nickel
where: World Mine Production and Reserves table, 2025e column, shares calculated by Space Mushroom against the printed world total of 3,900,000 t (not printed as shares); Recycling; Substitutes
- subject: Chromium
abundance: World resources are greater than 12 billion tons of shipping-grade chromite (USGS)
producers:
- country: South Africa
share_percent: 45.1
year: 2025
- country: Turkey
share_percent: 17.6
year: 2025
- country: Kazakhstan
share_percent: 13.7
year: 2025
- country: India
share_percent: 5.9
year: 2025
recycling: In 2025, recycled chromium in reported stainless-steel scrap receipts accounted for 21% of apparent consumption (USGS).
substitutes:
- Chromium has no substitute in stainless steel, the leading end use, or in superalloys, the major strategic end use (USGS).
source: usgs-mcs2026-chromium
where: World Mine Production and Reserves table, 2025e column, shares calculated by Space Mushroom against the printed world total of 51,000 thousand t; Recycling; Substitutes
- subject: Molybdenum
abundance: Identified resources in the United States are about 5.4 million tons and, in the rest of the world, about 20 million tons (USGS)
producers:
- country: China
share_percent: 37.3
year: 2025
- country: Chile
share_percent: 16.2
year: 2025
- country: United States
share_percent: 15.4
year: 2025
- country: Peru
share_percent: 15
year: 2025
- country: Mexico
share_percent: 6.5
year: 2025
recycling: Molybdenum is recycled as a component of catalysts, ferrous scrap and superalloy scrap; the recycled amount may be as much as 30% of apparent supply (USGS).
substitutes:
- There is little substitution for molybdenum in steels and cast irons. Potential substitutes in alloy steels include boron, chromium, niobium and vanadium (USGS).
source: usgs-mcs2026-molybdenum
where: World Mine Production and Reserves table, 2025e column, shares calculated by Space Mushroom against the printed world total of 260,000 t; Recycling; Substitutes
- subject: Niobium
abundance: World resources of niobium are more than adequate to supply projected needs (USGS)
producers:
- country: Brazil
share_percent: 92.9
year: 2025
- country: Canada
share_percent: 5.4
year: 2025
recycling: Niobium scrap recovery was negligible; recycled niobium may have been as much as 20% of apparent consumption (USGS).
substitutes:
- Ceramic matrix composites, molybdenum, tantalum and tungsten can replace niobium in high-temperature superalloy applications, with a performance loss or higher cost (USGS).
source: usgs-mcs2026-niobium
where: World Mine Production and Reserves table, 2025e column (niobium content), shares calculated by Space Mushroom against the printed world total of 112,000 t; Recycling; Substitutes
media: []
documents:
- title: Special Metals INCONEL alloy 625 datasheet (2013 Aug 13)
type: datasheet
url: https://www.specialmetals.com/documents/technical-bulletins/inconel/inconel-alloy-625.pdf
year: 2013
- title: ATI 625 Alloy Technical Data Sheet, version 1 (3/4/2012), Allvac version
type: datasheet
url: https://www.atimaterials.com/Products/Documents/datasheets/nickel-cobalt/nickel-based/ati_625_allvac_version_tds_en_v1.pdf
year: 2012
- title: ATI 625 Nickel-Based Alloy product page (plate minimums, Grade 1 and Grade 2 condition statement)
type: datasheet
url: https://www.atimaterials.com/Products/ati-625
- title: 'USGS Mineral Commodity Summaries 2026: Nickel'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-nickel.pdf
year: 2026
- title: 'USGS Mineral Commodity Summaries 2026: Chromium'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-chromium.pdf
year: 2026
- title: 'USGS Mineral Commodity Summaries 2026: Molybdenum'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-molybdenum.pdf
year: 2026
- title: 'USGS Mineral Commodity Summaries 2026: Niobium (Columbium)'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-niobium.pdf
year: 2026
- title: 'PubChem: Nickel (CID 935), GHS classification (PUG View JSON)'
type: database
url: https://pubchem.ncbi.nlm.nih.gov/rest/pug_view/data/compound/935/JSON?heading=GHS+Classification
- title: Renishaw safety data sheet, Inconel 625 metal powder (document H-5800-3483-02-A_EN, SDS date 1/27/2023)
type: sds
url: https://www.renishaw.com/media/pdf/en/ec20c331517e4b0ba85c69455df4e8f3.pdf
year: 2023
gaps:
- Grade 2 (solution-annealed) ASTM B 443 and B 446 minimum strengths were not read on a fetched standard or manufacturer page. The solution-annealed values here are Special Metals ranges and the Table 8 anneal results.
- The ASTM standard texts are paywalled and the ASTM B 443 page did not load, so the designations come from the datasheets and the Wikipedia infobox.
- The EN steel name NiCr22Mo9Nb is not printed in any source read here, so only W.Nr. 2.4856 and EN 10095 are listed.
- No numeric minimum service temperature is printed. The datasheet says service from cryogenic temperatures, so min_service_temp is left out.
- Creep and rupture curves (datasheet Figures 11 to 14), elevated-temperature tensile curves (Figures 3 to 5) and the scaling chart (Figure 15) are graphs and were not read as numbers.
- 'Charpy impact at -320 F (Table 7) and Brinell hardness (Table 5) are printed but not added: the impact results are triplicate values with no canonical name, and hardness has no canonical name.'
- The USGS 2026 summaries for nickel, chromium, molybdenum and niobium print no critical-mineral list status (nickel is mentioned only in an executive order), so there are no critical_lists entries.
- The Renishaw SDS covers the powder form only. No safety data sheet for solid Inconel 625 stock was read, so the hazards for solid alloy rely on the nickel record.
- No quantitative corrosion test (critical pitting temperature, ASTM G48, corrosion rate or SCC threshold) was read in this run. The corrosion entries are qualitative, from the Special Metals and ATI datasheets.
- The Special Metals datasheet is dated 2013 and the ATI sheet is dated 2012 (Allvac version). The USGS production figures are 2025 estimates, and the shares are calculated from printed tonnages.
- Table 5 values are composites for product sizes up to 4 in and are not specification values. No size-specific data were read.
- ATI notes that lower-carbon versions can be age hardened (aged up to 120 hours at 1050 to 1350 F). No property data for that version were read, so it is not covered.
- The ATI bar (AMS 5666) minimums are not used because the bar rows do not state the condition.
sources:
sm625:
title: INCONEL alloy 625 datasheet, Special Metals Corporation
id: Special Metals Corporation, copyright 2013 (Aug 13)
url: https://www.specialmetals.com/documents/technical-bulletins/inconel/inconel-alloy-625.pdf
year: 2013
kind: datasheet
license: Special Metals terms (cited, not reproduced)
ati-tds:
title: ATI 625 Alloy Technical Data Sheet (Allvac version)
id: ATI Allegheny Technologies, version 1 (3/4/2012)
url: https://www.atimaterials.com/Products/Documents/datasheets/nickel-cobalt/nickel-based/ati_625_allvac_version_tds_en_v1.pdf
year: 2012
kind: datasheet
license: ATI terms (cited, not reproduced)
ati-page:
title: ATI 625 Nickel-Based Alloy product page
id: ATI product page, read in this run (2026-10-24)
url: https://www.atimaterials.com/Products/ati-625
kind: web
license: ATI terms (cited, not reproduced)
usgs-mcs2026-nickel:
title: 'Mineral Commodity Summaries 2026: Nickel'
id: USGS, Mineral Commodity Summaries 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-nickel.pdf
year: 2026
kind: report
license: US Government work (public domain)
usgs-mcs2026-chromium:
title: 'Mineral Commodity Summaries 2026: Chromium'
id: USGS, Mineral Commodity Summaries 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-chromium.pdf
year: 2026
kind: report
license: US Government work (public domain)
usgs-mcs2026-molybdenum:
title: 'Mineral Commodity Summaries 2026: Molybdenum'
id: USGS, Mineral Commodity Summaries 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-molybdenum.pdf
year: 2026
kind: report
license: US Government work (public domain)
usgs-mcs2026-niobium:
title: 'Mineral Commodity Summaries 2026: Niobium (Columbium)'
id: USGS, Mineral Commodity Summaries 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-niobium.pdf
year: 2026
kind: report
license: US Government work (public domain)
pubchem-nickel:
title: Nickel, PubChem CID 935, GHS classification (aggregated ECHA C&L notifications)
id: PubChem CID 935
url: https://pubchem.ncbi.nlm.nih.gov/rest/pug_view/data/compound/935/JSON?heading=GHS+Classification
kind: database
license: PubChem (NIH, public domain)
renishaw-sds:
title: Renishaw safety data sheet, Inconel 625 metal powder
id: Renishaw plc, document H-5800-3483-02-A_EN, SDS date 1/27/2023, version 1.0
url: https://www.renishaw.com/media/pdf/en/ec20c331517e4b0ba85c69455df4e8f3.pdf
year: 2023
kind: datasheet
license: Renishaw terms (cited, not reproduced)
wiki625:
title: Inconel 625
id: Wikipedia, English article (read in this run, 2026-10-24)
url: https://en.wikipedia.org/wiki/Inconel_625
kind: web
license: CC BY-SA 4.0
license: CC-BY-4.0
updated: '2026-10-24'
review:
status: draft
method: assistant
checked_values: 37
unreachable: 0
caveats: 15
note: Written by an AI assistant on 2026-10-24 from the Special Metals 625 datasheet (2013), the ATI 625 TDS (2012) and product page, the Renishaw powder SDS, the USGS 2026 nickel, chromium, molybdenum and niobium summaries, the PubChem nickel GHS record and Wikipedia (designations, trade names and phase data only). Every number was read from a page fetched in this run; none came from search snippets. The file structure is copied from the Inconel 718 sibling (inconel-718), which the compare paragraph links to.
story:
recipe:
line: 'Inconel 625 is a solid-solution nickel-chromium-molybdenum-niobium alloy, made by vacuum induction melting followed by electroslag remelting (ATI TDS). Special Metals gives the limiting composition in weight percent: at least 58 percent nickel, 20 to 23 percent chromium, 8 to 10 percent molybdenum, 3.15 to 4.15 percent niobium plus tantalum, and up to 5 percent iron, with small maximum limits on the other elements.'
parts:
- name: Nickel
symbol: Ni
share_percent: 58
share_note: minimum (the matrix)
role: Matrix of the alloy, a face-centred-cubic solid solution
source: sm625
where: Table 1, Limiting Chemical Composition
- name: Chromium
symbol: Cr
share_percent: 20
share_high: 23
role: Gives resistance to oxidising chemicals and to oxidation and scaling at high temperature
source: sm625
where: Table 1, Limiting Chemical Composition
- name: Molybdenum
symbol: Mo
share_percent: 8
share_high: 10
role: Stiffens the matrix and makes the alloy very resistant to pitting and crevice corrosion
source: sm625
where: Table 1, Limiting Chemical Composition
- name: Niobium plus tantalum
symbol: Nb
share_percent: 3.15
share_high: 4.15
role: Stiffens the matrix, which is the main strengthening effect, and stabilises the alloy against sensitisation during welding
source: sm625
where: Table 1, Limiting Chemical Composition
- name: Iron
symbol: Fe
share_note: 5.0 maximum
role: Residual element, limited to 5.0 percent
source: sm625
where: Table 1, Limiting Chemical Composition
- name: Cobalt
symbol: Co
share_note: 1.0 maximum, if determined
role: Residual element
source: sm625
where: Table 1, footnote a
- name: Minor elements
share_note: C 0.10, Mn 0.50, Si 0.50, Al 0.40, Ti 0.40, P 0.015 and S 0.015 maximum (wt%)
role: Residual limits. The datasheet says precipitation-hardening treatments are not required.
source: sm625
where: Table 1; Introduction
risk_groups:
- title: For people
level: 2
verdict: Solid metal flagged by the nickel record; powder is Danger
lead: No GHS classification was read for the solid alloy. The hazard flags come from the PubChem nickel record (nickel is about 58 percent of this alloy) and from the Renishaw safety data sheet for the metal powder.
points:
- label: Solid metal
line: The PubChem aggregated nickel record lists skin sensitisation (H317, 99.9 percent of reports), suspected cancer (H351, 72.9 percent) and organ damage from prolonged exposure (H372, 99.7 percent).
- label: Powder and dust
line: The Renishaw safety data sheet for the metal powder carries the signal word Danger and the codes H317, H334, H350, H360F and H372, and says the powder may form an explosible dust-air mixture.
- title: If a part is held in the wrong temperature range
lead: These results come from the datasheets and the Wikipedia summary of phase behaviour, not from field incidents.
points:
- label: Long exposure near 1200 F
line: After 2000 hours at 1200 F, room-temperature tensile strength rises from 140.0 to 176.0 ksi and elongation falls from 54 to 30 percent (Special Metals Table 6).
- label: Precipitates from 923 to 1148 K
line: Wikipedia says precipitates form in the range 923 to 1148 K that are detrimental to creep properties, and that delta phase begins to form at 998 K.
- title: Handling and heat treatment
points:
- label: Forming
line: Hot forming uses a furnace held at no more than 2150 F, with heavy forging from 2150 to 1850 F and lighter reductions down to 1700 F (Special Metals).
- label: Scale removal
line: Heating scale is tightly adherent, so a fused-salt bath before pickling is usually recommended (Special Metals).
why: Inconel 625 was first developed as a steam-line piping material and has since spread to chemical processing, marine and nuclear equipment and aerospace ducting (Wikipedia; ATI). Its strength comes from molybdenum and niobium stiffening the nickel-chromium matrix, so it needs no precipitation-hardening step (Special Metals). That combination gives resistance to a wide range of corrosive media, including chloride stress-corrosion cracking, and good oxidation resistance (Special Metals; ATI).
uses:
- where: Rocket engines and fuel lines
line: Special Metals lists thrust-chamber tubing for rocket engines, fuel and hydraulic line tubing, engine exhaust systems and combustion-system transition liners among its aerospace uses.
- where: Aircraft structures and ducting
line: Aircraft ducting systems, resistance-welded honeycomb structures housing engine controls, and turbine shroud rings are named in the datasheet. ATI says the alloy is widely used in aerospace for airframe and jet engine applications.
- where: Heat exchangers in environmental control systems
line: Special Metals lists heat-exchanger tubing in environmental control systems among its aerospace uses.
- where: Chemical plant and marine service
line: Special Metals names bubble caps, tubing, reaction vessels, distillation columns, heat exchangers and valves for chemical processing, and wire rope for mooring cables, propeller blades and sheathing for undersea cables for marine service.
can_do:
- label: Strength in the annealed grade
line: Annealed (grade 1) rod, bar and plate give 60 to 95 ksi yield and 120 to 150 ksi tensile strength at room temperature (Special Metals Table 5, composite ranges).
- label: Lower strength in the solution-annealed grade
line: Solution-annealed (grade 2) rod, bar and plate give 42 to 60 ksi yield and 105 to 130 ksi tensile strength, so the two grades differ in strength (Table 5).
- label: Stiffness
line: Young modulus is 207.5 GPa for the annealed grade and 204.8 GPa for the solution-annealed grade at 21 C (Table 4).
- label: Oxidation at high temperature
line: The datasheet gives service up to 1800 F (982 C), and ATI rates oxidation resistance as excellent up to 2,000 F (1,093 C).
- label: Corrosion in mild and severe media
line: Almost no attack in the atmosphere, fresh and sea water, neutral salts and alkaline media, and freedom from chloride-ion stress-corrosion cracking (Special Metals).
compare: Compare with [Inconel 718](/profiles/inconel-718/), the age-hardened sibling. Its strength comes from precipitates formed in heat treatment, while Inconel 625 is solid-solution strengthened and the Special Metals datasheet says no precipitation-hardening treatment is required. The 718 profile carries its own precipitation and heat-treatment data.
compare_rows:
- label: Density
benchmark: density
scope: material
- label: Stiffness
benchmark: elastic_modulus
scope: material
- label: Melting range
benchmark: melting_point
scope: material
handling:
- Anneal hot- or cold-formed parts at 1700 to 1900 F for times set by thickness (annealed, grade 1). Solution treat at 2000 to 2200 F where optimum creep-rupture strength is needed (solution-annealed, grade 2) (Special Metals). ATI gives 1600 to 1900 F for the anneal.
- Remove sulphur-bearing lubricants before heat treating and pickling (ATI).
- Remove heating scale with a fused-salt bath before pickling (Special Metals).
- Hot form in a furnace held at no more than 2150 F, with heavy forging from 2150 to 1850 F and lighter reductions to 1700 F. Use uniform reductions to avoid duplex grain (Special Metals).
- Stress-relieve cold-drawn material at 1100 to 1400 F. Stress relief is virtually complete at 1600 F (Special Metals).
- For welds, use INCONEL Filler Metal 625 or Welding Electrode 112. The datasheet says the weld metal needs no postweld heat treatment to keep its strength and ductility (Special Metals).
good_for:
- Corrosion-resistant parts that must also carry strength, such as chemical plant equipment, marine hardware and sea-water service (Special Metals).
- Hot ducting and exhaust parts up to 1800 F (982 C) where oxidation resistance matters (Special Metals; ATI).
- Welded assemblies that need corrosion resistance matched to the base alloy (Special Metals).
watch_out:
- Long exposure near 1200 F hardens the annealed alloy and drops room-temperature elongation from 54 to 30 percent after 2000 hours (Special Metals Table 6).
- The annealed (grade 1) and solution-annealed (grade 2) grades differ in strength, so the grade must be stated on any design basis (Special Metals; ATI).
- Strength ranges are composites for product sizes up to 4 in and are not specification values (Special Metals).
- Notched fatigue strength is far below smooth fatigue strength, 35,000 psi against 90,000 psi (Special Metals).
- The corrosion entries are qualitative. No corrosion rate or critical pitting temperature was read in this run.
verdict: Inconel 625 is a corrosion-resistant solid-solution alloy for strength up to 1800 F. Its annealed and solution-annealed grades differ in strength, so state the grade for each design, and keep long exposures near 1200 F in mind.
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.
| # | Source | Type | Year | Used for |
|---|---|---|---|---|
| INCONEL alloy 625 datasheet, Special Metals Corporation | datasheet | 2013 | 56 values | |
| ATI 625 Alloy Technical Data Sheet (Allvac version) | datasheet | 2012 | 2 values | |
| ATI 625 Nickel-Based Alloy product page | web | 3 values | ||
| Mineral Commodity Summaries 2026: Nickel | report | 2026 | 1 value | |
| Mineral Commodity Summaries 2026: Chromium | report | 2026 | 1 value | |
| Mineral Commodity Summaries 2026: Molybdenum | report | 2026 | 1 value | |
| Mineral Commodity Summaries 2026: Niobium (Columbium) | report | 2026 | 1 value | |
| Nickel, PubChem CID 935, GHS classification (aggregated ECHA C&L notifications) | database | 1 value | ||
| Renishaw safety data sheet, Inconel 625 metal powder | datasheet | 2023 | 3 values | |
| Inconel 625 | web | 2 values |