Alloy 42 FeNi42
Fe-42Ni, nominal: a binary nickel-iron alloy with 41 % nickel minimum (42 % nominal) and iron as the balance
Also known as UNS K94100, EN 1.3917, DIN 17745, AFNOR NF A54-301, ASTM F30, ASTM F29 · 3 more
Alloy 42 is a binary nickel-iron alloy with 42 % nickel (UNS K94100, Werkstoff Nr.
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Low expansion
4.0 to 4.7 ppm/K
Strength when annealed
490 MPa tensile, 250 MPa yield
Stiffness
150 GPa
Recipe, share of the weight
- Ni 41%Nickel
- Fe not statedIron
- C not statedCarbon
- Mn not statedManganese
- Si not statedSilicon
- Cr not statedChromium
- P not statedPhosphorus
- S not statedSulphur
- Al not statedAluminium
Best for
Glass-to-metal and ceramic-to-metal seals, and lead frames for integrated circuits, where expansion must stay low up to 300 °C
Weakest at
Strength and corrosion data: no corrosion test was found, and the sources disagree on yield strength, tensile strength and elongation
Risk at a glance
- People None found. Nickel content: skin sensitiser, suspected carcinogen
- If it fails Moderate. Dimensional drift from cold work
- Corrosion Low. The supplier describes Alloy 42 as strongly resistant to oxidation and corrosion, with no test data given.
Quick facts: FeNi42
| Property | Value | Basis |
|---|---|---|
| Density | 8.11 to 8.15 g/cm³ | 3 sourced values across conditions |
| Yield strength | 250 to 300 MPa | 3 sourced values across conditions |
| Tensile strength | 490 to 517 MPa | 3 sourced values across conditions |
| Young's modulus | 145 to 150 GPa | 3 sourced values across conditions |
| Thermal conductivity | 10.5 to 12.5 W/(m·K) | 2 sourced values across conditions |
| Thermal expansion (CTE) | 4 to 7.4 ppm/K | 3 sourced values across conditions |
| Melting point | 1,425 to 1,435 °C | 3 sourced values across conditions |
| Specific heat | 500 J/(kg·K) | 1 sourced value |
| Electrical resistivity | 6.1e-7 to 6.6e-7 Ω·m | 2 sourced values across conditions |
What is the density of Alloy 42 (FeNi42)?
Alloy 42 (FeNi42) has a density of 8.11 to 8.15 g/cm³. The range covers 3 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the thermal conductivity of Alloy 42 (FeNi42)?
Alloy 42 (FeNi42) has a thermal conductivity of 10.5 to 12.5 W/(m·K). The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the coefficient of thermal expansion of Alloy 42 (FeNi42)?
Alloy 42 (FeNi42) has a coefficient of thermal expansion of 4 to 7.4 ppm/K. The range covers 3 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the melting point of Alloy 42 (FeNi42)?
Alloy 42 (FeNi42) has a melting point of 1,425 to 1,435 °C. The range covers 3 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the yield strength of Alloy 42 (FeNi42)?
Alloy 42 (FeNi42) has a yield strength of 250 to 300 MPa. The range covers 3 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What are the other names and codes for Alloy 42 (FeNi42)?
Alloy 42 (FeNi42) is also written as UNS K94100, EN 1.3917, DIN 17745, AFNOR NF A54-301, ASTM F30, ASTM F29. Each code is printed in the source listed beside it in the designations table.
What is Alloy 42 (FeNi42) used for?
Uses recorded in the sources include Semiconductor lead frames in integrated circuits; Glass-to-metal seals in electronic tubes and lamps; Tooling for aerospace composites.
Why it exists
Alloy 42 is a nickel-iron alloy with about 42 % nickel. Its thermal expansion is low and nearly constant from room temperature to about 300 °C, which is why it is used where it must seal to glass or ceramic, or hold a dimension while the temperature changes. The sources name lead frames in integrated circuits, glass-to-metal seals in electronic tubes and lamps, and tooling that shapes aerospace composites as its uses.
Where it's used
Electronic packages
Aircraft Materials says Alloy 42 is used for semiconductor lead frames in integrated circuits. High Temp Metals says it has been used for glass-to-metal seals in electronic tubes and lamps.
Composite tooling
Special Metals says NILO alloy 42 is used for tooling for aerospace composites, and NeoNickel lists composite tooling among its applications.
Cryogenic and bimetal parts
NeoNickel lists cryogenic components and liquid-gas storage tanks. Special Metals lists its use in thermostatic bi-metal strip as the low-expansion component.
Recipe
Fe-42Ni, nominal: a binary nickel-iron alloy with 41 % nickel minimum (42 % nominal) and iron as the balance; carbon 0.05 % maximum, manganese 0.8 % maximum, silicon 0.03 % maximum, chromium 0.25 % maximum, phosphorus and sulphur 0.025 % maximum, aluminium 0.1 % maximum (NeoNickel chemical analysis)
Alloy 42 is a binary nickel-iron alloy. It is about 42 % nickel with iron as the balance, plus small maximum limits on carbon, manganese, silicon, chromium, phosphorus, sulphur and aluminium (Special Metals; NeoNickel).
| Ingredient | Share of the weight | What it does |
|---|---|---|
| Nickel Ni | 41% | 41 % minimum in the chemical limits; the nominal 42 % gives the alloy its name (NeoNickel; Special Metals Table 1). |
| Iron Fe | not stated | The balance of the composition in every limit table read. |
| Carbon C | not stated | Maximum 0.05 % (Aircraft Materials; High Temp Metals). |
| Manganese Mn | not stated | Maximum 0.8 % (NeoNickel). |
| Silicon Si | not stated | Maximum 0.03 % (NeoNickel). |
| Chromium Cr | not stated | Maximum 0.25 % (NeoNickel). |
| Phosphorus P | not stated | Maximum 0.025 % (NeoNickel). |
| Sulphur S | not stated | Maximum 0.025 % (NeoNickel). |
| Aluminium Al | not stated | Maximum 0.1 % (NeoNickel). |
Weight shares are as printed in the sources.
What it can do
Low expansion
4.0 to 4.7 ppm/K
measured
Holds a low, nearly constant expansion from cryogenic temperatures up to about 300 °C (NeoNickel), and NeoNickel prints a mean of 4.0 to 4.7 ppm/K from 30 to 300 °C.
Strength when annealed
490 MPa tensile, 250 MPa yield
measured
Annealed bar has a tensile strength of 490 MPa and a yield strength of 250 MPa at 20 °C (Special Metals Table 12).
Stiffness
150 GPa
measured
Elastic modulus of 150 GPa (Special Metals Table 16), against 148 GPa at 20 °C on the NeoNickel page.
How it compares
Alloy 42 has a density of 8.11 g/cm3 in Special Metals' table and 8.12 g/cm3 in NeoNickel's, so the two sources differ only slightly. On expansion, Special Metals' typical table gives a mean linear coefficient of 5.3 ppm/K from 20 to 300 °C, while NeoNickel gives 4.0 to 4.7 ppm/K from 30 to 300 °C. The sources disagree on this figure, so the conditions of each value matter more than the single number. The table compares the three properties most often used to choose the alloy.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | FeNi42 | IN718 (UNS N07718) | IN625 (UNS N06625) | FeNi36 | Ni-Mo | C-22 | C-276 (UNS N10276) | X (UNS N06002) | UNS N07214 | H230 (UNS N06230) | UNS N08800 | Alloy 825 (UNS N08825) | Alloy 600 (UNS N06600, W.Nr. 2.4816) | Alloy 601 | Alloy 617 | X-750 (UNS N07750) | Fe-Ni-Co | Alloy 400 (UNS N04400) | K-500 | Ni | Ni3Al, NiAl | NiBe2 | Ni-alloys | UNS N07090 (W. Nr. 2.4632) | UNS N07001 |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Thermal behavior and safety | |||||||||||||||||||||||||
| Melting range, Alloy 42 (NeoNickel) | 1425 to 1435 °C3 | 1260 °C | 1290 to 1350 °C | 1427 °C | 1370 to 1418 °C | 1357 to 1399 °C | 1323 to 1371 °C | 1260 to 1355 °C | 1355 to 1400 °C | 1301 to 1371 °C | 1357 to 1385 °C | 1370 to 1400 °C | 1354 to 1413 °C | 1360 to 1411 °C | 1330 to 1380 °C | 1393 to 1427 °C | 1450 °C | 1300 to 1350 °C | 1315 to 1350 °C | 1455 °C | no data | 1195 to 1325 °C | 1425 °C | 1370 °C | 1330 to 1360 °C |
| Melting point, NILO alloy 42 (Special Metals) | 1435 °C4 | 1260 °C | 1290 to 1350 °C | 1427 °C | 1370 to 1418 °C | 1357 to 1399 °C | 1323 to 1371 °C | 1260 to 1355 °C | 1355 to 1400 °C | 1301 to 1371 °C | 1357 to 1385 °C | 1370 to 1400 °C | 1354 to 1413 °C | 1360 to 1411 °C | 1330 to 1380 °C | 1393 to 1427 °C | 1450 °C | 1300 to 1350 °C | 1315 to 1350 °C | 1455 °C | no data | 1195 to 1325 °C | 1425 °C | 1370 °C | 1330 to 1360 °C |
| Melting point, Alloy 42 (High Temp Metals)Value printed in a supplier technical data sheet | 1427 °C | 1260 °C | 1290 to 1350 °C | 1427 °C | 1370 to 1418 °C | 1357 to 1399 °C | 1323 to 1371 °C | 1260 to 1355 °C | 1355 to 1400 °C | 1301 to 1371 °C | 1357 to 1385 °C | 1370 to 1400 °C | 1354 to 1413 °C | 1360 to 1411 °C | 1330 to 1380 °C | 1393 to 1427 °C | 1450 °C | 1300 to 1350 °C | 1315 to 1350 °C | 1455 °C | no data | 1195 to 1325 °C | 1425 °C | 1370 °C | 1330 to 1360 °C |
| Thermal conductivity, NILO alloy 42 (Special Metals) | 10.5 W/m°C6 | 79 BTU·in/ft²·h·°F | 9.8 W/m°C | 72.85 Btu·in/(hr·ft²·°F) | 11.2 W/m.°C | 10.1 W/(m·K) | 10.5 W/m.°C | 9.2 W/(m·K) | 12 W/m-°C | 8.9 W/(m·°C) | 11.5 W/m°C | 11.1 W/(m·K) | 14.9 W/(m·K) | 11.2 W/(m·K) | 13.4 W/(m·K) | 83 Btu/in./hr/sq ft/°F | 17.5 W/m °K | 22 W/m°C | 17.5 W/m °C | 70.3 W/(m·K) | no data | 48 W/(m·K) | 13 W/(m·K) | 11.47 W/(m·K) | 19.1 W/(m·°C) |
| Thermal conductivity, Alloy 42 (NeoNickel) | 10.7 W/m-K7 | 79 BTU·in/ft²·h·°F | 9.8 W/m°C | 72.85 Btu·in/(hr·ft²·°F) | 11.2 W/m.°C | 10.1 W/(m·K) | 10.5 W/m.°C | 9.2 W/(m·K) | 12 W/m-°C | 8.9 W/(m·°C) | 11.5 W/m°C | 11.1 W/(m·K) | 14.9 W/(m·K) | 11.2 W/(m·K) | 13.4 W/(m·K) | 83 Btu/in./hr/sq ft/°F | 17.5 W/m °K | 22 W/m°C | 17.5 W/m °C | 70.3 W/(m·K) | no data | 48 W/(m·K) | 13 W/(m·K) | 11.47 W/(m·K) | 19.1 W/(m·°C) |
| Specific heat, Alloy 42 (High Temp Metals)Value printed in a supplier technical data sheet | 0.5 kJ/kg-K | 435 J/kg °C | 410 J/(kg·K) | 515 J/(kg·K) | 373 J/kg.°C | 410 J/(kg·K) | 427 J/kg.°C | 486 J/(kg·K) | 452 J/kg-°C | 397 J/kg·°C | 460 J/kg·°C | 440 J/(kg·K) | 444 J/kg °C | 448 J/(kg·K) | 419 J/(kg·K) | 0.103 Btu/lb/°F | 500 J/(kg. K) | 427 J/kg°C | 419 J/kg °C | 456 J/(kg·K) | no data | no data | 500 J/(kg·K) | 446 J/(kg·K) | no data |
| Thermal conductivity, 1.3917 Alloy 42 (METALCOR) | 12.5 W/m K22 | 79 BTU·in/ft²·h·°F | 9.8 W/m°C | 72.85 Btu·in/(hr·ft²·°F) | 11.2 W/m.°C | 10.1 W/(m·K) | 10.5 W/m.°C | 9.2 W/(m·K) | 12 W/m-°C | 8.9 W/(m·°C) | 11.5 W/m°C | 11.1 W/(m·K) | 14.9 W/(m·K) | 11.2 W/(m·K) | 13.4 W/(m·K) | 83 Btu/in./hr/sq ft/°F | 17.5 W/m °K | 22 W/m°C | 17.5 W/m °C | 70.3 W/(m·K) | no data | 48 W/(m·K) | 13 W/(m·K) | 11.47 W/(m·K) | 19.1 W/(m·°C) |
| Physical and electrical | |||||||||||||||||||||||||
| Density, NILO alloy 42 (Special Metals) | 8.11 g/cm³1 | 0.297 lb/in3 | 8.44 g/cm³ | 8.05 g/cm³ | 9.22 g/cm³ | 8.69 g/cm³ | 8.89 g/cm³ | 8.22 g/cm³ | 8.05 g/cm³ | 8.97 g/cm³ | 7.94 g/cm³ | 8.14 g/cm³ | 0.306 lb/in3 | 8.11 Mg/m3 | 8.36 g/cm³ | 8.28 g/cm³ | 8.36 g/cm³ | 8.8 g/cm³ | 8.45 g/cm³ | 8.89 g/cm³ | 7.5 g/cm³ | 8.27 g/cm³ | 8.2 g/cm³ | 8.18 g/cm³ | 8.19 g/cm³ |
| Density, Alloy 42 (NeoNickel) | 8.12 g/cm³2 | 0.297 lb/in3 | 8.44 g/cm³ | 8.05 g/cm³ | 9.22 g/cm³ | 8.69 g/cm³ | 8.89 g/cm³ | 8.22 g/cm³ | 8.05 g/cm³ | 8.97 g/cm³ | 7.94 g/cm³ | 8.14 g/cm³ | 0.306 lb/in3 | 8.11 Mg/m3 | 8.36 g/cm³ | 8.28 g/cm³ | 8.36 g/cm³ | 8.8 g/cm³ | 8.45 g/cm³ | 8.89 g/cm³ | 7.5 g/cm³ | 8.27 g/cm³ | 8.2 g/cm³ | 8.18 g/cm³ | 8.19 g/cm³ |
| Electrical resistivity at 20 °C, NILO alloy 42 (Special Metals) | 61 microhm-cm19 | 725 ohm circ mil/ft | 129 µΩ-cm | 84 µΩ·cm | 1.37 μohm.m | 1.14 µΩ·m | 1.23 μohm.m | 114.8 µohm-cm | 135.9 µohm-cm | 125 µohm-m | 0.989 µΩ·m | 112 µΩ·cm | 1.03 µΩ·m | 1.18 µΩ·m | 1.22×10^-4 Ω·cm | 731 ohm circ mil/ft | 49 μΩcm | 0.511 µΩ·m | 0.615 µΩ·m | 0.096 µΩ·m | no data | < 28.7 µΩ·cm | 45 µΩ·cm | 1.18 µΩ·m | 1.24 µΩ·m |
| Electrical resistivity, Alloy 42 (High Temp Metals)Value printed in a supplier technical data sheet | 66 microhm-cm20 | 725 ohm circ mil/ft | 129 µΩ-cm | 84 µΩ·cm | 1.37 μohm.m | 1.14 µΩ·m | 1.23 μohm.m | 114.8 µohm-cm | 135.9 µohm-cm | 125 µohm-m | 0.989 µΩ·m | 112 µΩ·cm | 1.03 µΩ·m | 1.18 µΩ·m | 1.22×10^-4 Ω·cm | 731 ohm circ mil/ft | 49 μΩcm | 0.511 µΩ·m | 0.615 µΩ·m | 0.096 µΩ·m | no data | < 28.7 µΩ·cm | 45 µΩ·cm | 1.18 µΩ·m | 1.24 µΩ·m |
| Density, 1.3917 Alloy 42 (METALCOR) | 8.15 g/cm³21 | 0.297 lb/in3 | 8.44 g/cm³ | 8.05 g/cm³ | 9.22 g/cm³ | 8.69 g/cm³ | 8.89 g/cm³ | 8.22 g/cm³ | 8.05 g/cm³ | 8.97 g/cm³ | 7.94 g/cm³ | 8.14 g/cm³ | 0.306 lb/in3 | 8.11 Mg/m3 | 8.36 g/cm³ | 8.28 g/cm³ | 8.36 g/cm³ | 8.8 g/cm³ | 8.45 g/cm³ | 8.89 g/cm³ | 7.5 g/cm³ | 8.27 g/cm³ | 8.2 g/cm³ | 8.18 g/cm³ | 8.19 g/cm³ |
| Temperature behavior | |||||||||||||||||||||||||
| Curie temperature, Alloy 42 (NeoNickel) | 380 °C5 | -112 °C | < -196 °C | 279 °C | no data | no data | no data | no data | no data | no data | -115 °C | < -196 °C | -124 °C | no data | no data | no data | 435 °C | 21 to 49 °C | -65 °C | 360 °C | no data | no data | 450 °C | no data | no data |
| Other measurements | |||||||||||||||||||||||||
| Mean linear expansion, 20 to 300 °C, typical (Special Metals) | 5.3 ppm/K8 | 8.91 ppm/°F | 12.8 ppm/°C | 1.3 ppm/K | 10.6 μm/m.°C | 12.4 ppm/K | 11.2 μm/m.°C | 13.9 µm/(m·K) | 14.6 µm/m-°C | 11.8 ppm/K | 14.4 µm/m/°C | 13.9 ppm/K | 10.4 ppm/K | 13.75 µm/m/°C | 11.6 µm/(m·K) | 7 10-6 in./in./°F | 5.86 10-6/°C | 14.2 µm/m°C | 13.7 10-6/°C | 13.3 ppm/K | no data | 14.5 ppm/K | 8 ppm/K | 12.7 µm/(m·K) | 14.3 µm/m·°C |
| Mean linear expansion, 30 to 300 °C (NeoNickel) | 4 to 4.7 ppm/K9 | 8.91 ppm/°F | 12.8 ppm/°C | 1.3 ppm/K | 10.6 μm/m.°C | 12.4 ppm/K | 11.2 μm/m.°C | 13.9 µm/(m·K) | 14.6 µm/m-°C | 11.8 ppm/K | 14.4 µm/m/°C | 13.9 ppm/K | 10.4 ppm/K | 13.75 µm/m/°C | 11.6 µm/(m·K) | 7 10-6 in./in./°F | 5.86 10-6/°C | 14.2 µm/m°C | 13.7 10-6/°C | 13.3 ppm/K | no data | 14.5 ppm/K | 8 ppm/K | 12.7 µm/(m·K) | 14.3 µm/m·°C |
| Mean linear expansion, 30 to 450 °C (NeoNickel) | 6.7 to 7.4 ppm/K10 | 8.91 ppm/°F | 12.8 ppm/°C | 1.3 ppm/K | 10.6 μm/m.°C | 12.4 ppm/K | 11.2 μm/m.°C | 13.9 µm/(m·K) | 14.6 µm/m-°C | 11.8 ppm/K | 14.4 µm/m/°C | 13.9 ppm/K | 10.4 ppm/K | 13.75 µm/m/°C | 11.6 µm/(m·K) | 7 10-6 in./in./°F | 5.86 10-6/°C | 14.2 µm/m°C | 13.7 10-6/°C | 13.3 ppm/K | no data | 14.5 ppm/K | 8 ppm/K | 12.7 µm/(m·K) | 14.3 µm/m·°C |
| Elastic modulus, NILO alloy 42 (Special Metals) | 150 GPa11 | 29 ksi x 10^3 | 207.5 GPa | 140 GPa | 216 GPa | 206 GPa | 205 GPa | 205 GPa | 218 GPa | 209 GPa | 196.5 GPa | 196 GPa | 214 GPa | 206.5 GPa | 211 GPa | 31 10^3 ksi | 138 kN/mm2 | 26 10^3 ksi | 179 GPa | 205 GPa | 200 GPa | 195 to 210 GPa | no data | 204 GPa | 211 GPa |
| Elastic modulus at 20 °C, Alloy 42 (NeoNickel) | 148 GPa12 | 29 ksi x 10^3 | 207.5 GPa | 140 GPa | 216 GPa | 206 GPa | 205 GPa | 205 GPa | 218 GPa | 209 GPa | 196.5 GPa | 196 GPa | 214 GPa | 206.5 GPa | 211 GPa | 31 10^3 ksi | 138 kN/mm2 | 26 10^3 ksi | 179 GPa | 205 GPa | 200 GPa | 195 to 210 GPa | no data | 204 GPa | 211 GPa |
| Yield strength (0.2% offset), annealed bar at 20 °C (Special Metals) | 250 MPa13 | 171 ksi | 60 to 95 ksi | 40 ksi | 421 MPa | > 310 MPa | 356 MPa | 340 MPa | 577 MPa | 417 MPa | 250 MPa | 338 MPa | 170 to 345 MPa | 292 MPa | 340 MPa | > 105 ksi | > 200 N/mm2 | 25 to 50 ksi | 276 to 414 MPa | 105 to 210 MPa | no data | 280 to 480 MPa | 280 MPa | 752 MPa | 586 MPa |
| Yield strength (0.2% offset), annealed at room temperature (Aircraft Materials) | 250 MPa14 | 171 ksi | 60 to 95 ksi | 40 ksi | 421 MPa | > 310 MPa | 356 MPa | 340 MPa | 577 MPa | 417 MPa | 250 MPa | 338 MPa | 170 to 345 MPa | 292 MPa | 340 MPa | > 105 ksi | > 200 N/mm2 | 25 to 50 ksi | 276 to 414 MPa | 105 to 210 MPa | no data | 280 to 480 MPa | 280 MPa | 752 MPa | 586 MPa |
| Tensile strength, annealed bar at 20 °C (Special Metals) | 490 MPa15 | 201 ksi | 120 to 150 ksi | 65 ksi | 862 MPa | 690 to 950 MPa | 792 MPa | 760 MPa | 975 MPa | 837 MPa | 590 MPa | 662 MPa | 550 to 690 MPa | 675 MPa | 710 MPa | > 165 ksi | 450 to 585 N/mm2 | 75 to 90 ksi | 621 to 758 MPa | 380 to 520 MPa | 2300 MPa | 660 to 900 MPa | 500 MPa | 1175 MPa | 1027 MPa |
| Tensile strength, annealed material (High Temp Metals) | 517 MPa16 | 201 ksi | 120 to 150 ksi | 65 ksi | 862 MPa | 690 to 950 MPa | 792 MPa | 760 MPa | 975 MPa | 837 MPa | 590 MPa | 662 MPa | 550 to 690 MPa | 675 MPa | 710 MPa | > 165 ksi | 450 to 585 N/mm2 | 75 to 90 ksi | 621 to 758 MPa | 380 to 520 MPa | 2300 MPa | 660 to 900 MPa | 500 MPa | 1175 MPa | 1027 MPa |
| Elongation on 50 mm (2 in), annealed bar at 20 °C (Special Metals) | 43 %17 | 26 % | 30 to 60 % | 35 % | 53 % | > 45 % | 61 % | 48.9 % | 37.3 % | 47.3 % | 17 % | 45 % | 35 to 55 % | 46 % | 62 % | > 20 % | > 25 % | 35 to 60 % | 20 to 35 % | 40 to 55 % | no data | > 30 % | 35 % | 30 % | 43 % |
| Elongation in 2 in, annealed (High Temp Metals) | 30 %18 | 26 % | 30 to 60 % | 35 % | 53 % | > 45 % | 61 % | 48.9 % | 37.3 % | 47.3 % | 17 % | 45 % | 35 to 55 % | 46 % | 62 % | > 20 % | > 25 % | 35 to 60 % | 20 to 35 % | 40 to 55 % | no data | > 30 % | 35 % | 30 % | 43 % |
| Yield strength Rp (0.2% proof), lower limit at 20 °C (METALCOR) | > 300 N/mm223 | 171 ksi | 60 to 95 ksi | 40 ksi | 421 MPa | > 310 MPa | 356 MPa | 340 MPa | 577 MPa | 417 MPa | 250 MPa | 338 MPa | 170 to 345 MPa | 292 MPa | 340 MPa | > 105 ksi | > 200 N/mm2 | 25 to 50 ksi | 276 to 414 MPa | 105 to 210 MPa | no data | 280 to 480 MPa | 280 MPa | 752 MPa | 586 MPa |
| Tensile strength Rm, lower limit at 20 °C (METALCOR) | > 500 N/mm224 | 201 ksi | 120 to 150 ksi | 65 ksi | 862 MPa | 690 to 950 MPa | 792 MPa | 760 MPa | 975 MPa | 837 MPa | 590 MPa | 662 MPa | 550 to 690 MPa | 675 MPa | 710 MPa | > 165 ksi | 450 to 585 N/mm2 | 75 to 90 ksi | 621 to 758 MPa | 380 to 520 MPa | 2300 MPa | 660 to 900 MPa | 500 MPa | 1175 MPa | 1027 MPa |
| Modulus of elasticity, 1.3917 Alloy 42 (METALCOR) | 145 kN/mm225 | 29 ksi x 10^3 | 207.5 GPa | 140 GPa | 216 GPa | 206 GPa | 205 GPa | 205 GPa | 218 GPa | 209 GPa | 196.5 GPa | 196 GPa | 214 GPa | 206.5 GPa | 211 GPa | 31 10^3 ksi | 138 kN/mm2 | 26 10^3 ksi | 179 GPa | 205 GPa | 200 GPa | 195 to 210 GPa | no data | 204 GPa | 211 GPa |
Why choose it, and why not
Good for
- Low expansion to about 300 °C: 4.0 to 4.7 ppm/K from 30 to 300 °C (NeoNickel), for glass and ceramic seals.
- Lead frames and bimetal parts, where the alloy is named in both the Aircraft Materials and Special Metals sources.
Watch out for
- The sources disagree on expansion (5.3 against 4.0 to 4.7 ppm/K), on tensile strength (490 against 517 MPa) and on elongation (43 against 30 %).
- No corrosion test data were found, and the only corrosion statement is a qualitative supplier phrase.
- Alloy 42 is a nickel alloy, so its hazard data come from the nickel record.
Alloy 42 is a low-expansion nickel-iron alloy for glass seals, lead frames and composite tooling, with consistent density and modulus data. The expansion figures and strength values differ by source, and no flight or corrosion test data were found.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Other names and standards
The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.
| System | Codes |
|---|---|
| UNS | K94100 |
| EN | 1.3917 |
| DIN | 17745 |
| AFNOR | NF A54-301 (composition) |
| ASTM | F30 (sheet, strip, rod, bar, tubing and wire), F29 (wire), B753 (sheet and strip), F1684 (specification named by NeoNickel) |
| Trade name | Nilo 42 |
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Density, NILO alloy 42 (Special Metals) | Value printed in a Special Metals technical bulletin (publication SMC-031, Sept 2004) | temperature not stated in Table 2unit in source 0.293 lb/in3 | — |
| 2 | Density, Alloy 42 (NeoNickel) | Value printed in a stockist product page (NeoNickel) | temperature not stated | Differs from the 8.11 g/cm3 printed by Special Metals; both are kept. |
| 3 | Melting range, Alloy 42 (NeoNickel) | Range printed in a stockist product page (NeoNickel) | basis melting range as printedunit in source 1425°C - 1435°C | — |
| 4 | Melting point, NILO alloy 42 (Special Metals) | Value printed in a Special Metals technical bulletin, Table 3 | unit in source 2615 °F | Special Metals gives a single figure at the top of the NeoNickel range. |
| 5 | Curie temperature, Alloy 42 (NeoNickel) | Value printed in a stockist product page (NeoNickel) | basis as printed on the product page; no test method given | High Temp Metals prints the same 380 °C (715 °F). |
| 6 | Thermal conductivity, NILO alloy 42 (Special Metals) | Value printed in a Special Metals technical bulletin, Table 4 | temperature 20 °C (68 °F)unit in source W/m°C; 72.8 Btu in/ft2h °F | — |
| 7 | Thermal conductivity, Alloy 42 (NeoNickel) | Value printed in a stockist product page (NeoNickel) | temperature 20/100 °C, as printed | Special Metals gives 10.5 W/m°C at 20 °C; High Temp Metals prints 10.7 W/m-K at 20/100 °C too. |
| 8 | Mean linear expansion, 20 to 300 °C, typical (Special Metals) | Typical value printed in a Special Metals technical bulletin, Table 8 (not a guaranteed minimum or maximum) | temperature range 20 to 300 °C (68 to 572 °F)basis typical mean linear coefficient for NILO alloy 42 as printedunit in source 10-6/°C | Differs from the 4.0 to 4.7 ppm/K printed by NeoNickel and High Temp Metals for 30 to 300 °C; both are kept and the sources are not reconciled. |
| 9 | Mean linear expansion, 30 to 300 °C (NeoNickel) | Range printed on a stockist product page (NeoNickel); High Temp Metals prints the same range | temperature range 30 to 300 °Cunit in source 10-6/°C | — |
| 10 | Mean linear expansion, 30 to 450 °C (NeoNickel) | Range printed on a stockist product page (NeoNickel) | temperature range 30 to 450 °Cunit in source 10-6/°C | — |
| 11 | Elastic modulus, NILO alloy 42 (Special Metals) | Value printed in a Special Metals technical bulletin, Table 16 | temperature not stated in Table 16unit in source 21.8 x 10^3 ksi | — |
| 12 | Elastic modulus at 20 °C, Alloy 42 (NeoNickel) | Value printed in a stockist product page (NeoNickel) | temperature 20 °C | — |
| 13 | Yield strength (0.2% offset), annealed bar at 20 °C (Special Metals) | Value printed in a Special Metals technical bulletin, Table 12 | temper annealed, hot-rolled bartemperature 20 °C (68 °F)test 0.2% offsetunit in source 36.0 ksi | — |
| 14 | Yield strength (0.2% offset), annealed at room temperature (Aircraft Materials) | Value printed in a supplier technical data sheet (Typical Mechanical Properties table) | temper annealedtest 0.2% offsetunit in source 36,000 psi | — |
| 15 | Tensile strength, annealed bar at 20 °C (Special Metals) | Value printed in a Special Metals technical bulletin, Table 12 | temper annealed, hot-rolled bartemperature 20 °C (68 °F)unit in source 71.0 ksi | The same 490 MPa is printed by Aircraft Materials for annealed material; High Temp Metals prints 517 MPa. |
| 16 | Tensile strength, annealed material (High Temp Metals) | Typical value printed in a supplier technical data sheet | temper annealed, material as tested by the supplierunit in source 75 ksi | Differs from the 490 MPa printed by Special Metals and Aircraft Materials; both are kept. |
| 17 | Elongation on 50 mm (2 in), annealed bar at 20 °C (Special Metals) | Value printed in a Special Metals technical bulletin, Table 12 | temper annealed, hot-rolled bartemperature 20 °C (68 °F)gauge 50 mm (2 inch) | — |
| 18 | Elongation in 2 in, annealed (High Temp Metals) | Typical value printed in a supplier technical data sheet | temper annealedgauge 2 in | Differs from the 43 % printed by Special Metals; both are kept. |
| 19 | Electrical resistivity at 20 °C, NILO alloy 42 (Special Metals) | Value printed in a Special Metals technical bulletin, Table 6 | temperature 20 °C (68 °F)unit in source 61 microhm cm (367 ohm circ mil/ft) | — |
| 20 | Electrical resistivity, Alloy 42 (High Temp Metals) | — | temperature not statedunit in source 400 ohm-cir mil/ft | Differs from the 61 microhm-cm at 20 °C printed by Special Metals; both are kept. |
| 21 | Density, 1.3917 Alloy 42 (METALCOR) | Value printed in a METALCOR datasheet, Physical Properties 20°C table | temperature 20 °C | Third density figure for this alloy; Special Metals gives 8.11 g/cm3 and NeoNickel 8.12 g/cm3. All three are kept. |
| 22 | Thermal conductivity, 1.3917 Alloy 42 (METALCOR) | Value printed in a METALCOR datasheet, Physical Properties 20°C table | temperature 20 °C | Higher than the 10.5 W/m°C (Special Metals) and 10.7 W/m-K (NeoNickel) figures. All three are kept and not reconciled. |
| 23 | Yield strength Rp (0.2% proof), lower limit at 20 °C (METALCOR) | Lower limit printed in a METALCOR datasheet, Mechanical Properties 20°C table | temperature 20 °Ctest 0.2% proof (Rp) as printedbasis lower limit printed with the sign ≥ | A lower limit, not a typical value, so it is not directly comparable with the 250 MPa typical yield from Special Metals. Both are kept. |
| 24 | Tensile strength Rm, lower limit at 20 °C (METALCOR) | Lower limit printed in a METALCOR datasheet, Mechanical Properties 20°C table | temperature 20 °Cbasis lower limit printed with the sign ≥ | A lower limit, not a typical value. Special Metals prints 490 MPa typical and High Temp Metals 517 MPa; all are kept. |
| 25 | Modulus of elasticity, 1.3917 Alloy 42 (METALCOR) | Value printed in a METALCOR datasheet, Mechanical Properties 20°C table | temperature 20 °C | Lower than the 148 GPa (NeoNickel) and 150 GPa (Special Metals) figures. All three are kept. |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Air under standard service conditions | low | The supplier describes Alloy 42 as strongly resistant to oxidation and corrosion, with no test data given.1 |
| Annealing atmosphere at 850 to 1000 °C | not rated | Alloy 42 is annealed at 850 to 1000 °C in a protective atmosphere, and the bulletin gives no oxidation rate.2 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Air under standard service conditions | Studer describes the alloy as having strong resistance to oxidation and corrosion under standard service conditions. The page names no environment, exposure time, test standard or corrosion rate. | basis qualitative supplier statement; standard service conditions not definedtest none stated |
| 2 | Annealing atmosphere at 850 to 1000 °C | Special Metals says that NILO alloys 42 and 48 can be annealed at 850 to 1000 °C in a protective atmosphere. The bulletin does not give an oxide thickness, a scaling rate or the type of protective gas. | temperature range 850 to 1000 °C (1560 to 1830 °F)atmosphere protective atmosphere, type not named |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
No safety data sheet for Alloy 42 itself was read. The hazard data we hold are PubChem's record for nickel, and Alloy 42 is 41 % nickel minimum.
- The nickel record
- PubChem's nickel summary lists skin sensitisation, suspected cancer and harm to aquatic life. These are hazards of the element, not a test of the alloy.
- Dust and fume
- Machining, grinding and welding make metal dust and fume. Handle the material as a nickel-containing alloy and avoid breathing the dust.
If the alloy is heated
These instructions come from the suppliers' heat-treatment and forging advice, not from incident reports.
- Annealing
- Special Metals gives an annealing range of 850 to 1000 °C in a protective atmosphere for NILO alloys 42 and 48.
- Forging
- High Temp Metals advises a forging temperature of 2150/2200 °F and avoiding prolonged soaking, which can pick up sulphur from the furnace atmosphere.
Handling and fabrication
The fabrication advice below comes from the Special Metals bulletin and the High Temp Metals data sheet.
- Machining
- Machine in the annealed condition with high speed steel or tungsten carbide tipped tools.
- Welding
- For tooling welds, Special Metals introduced NILO Filler Metals CF42. MIG spray and submerged arc welding are not recommended for the NILO series.
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Dimensional drift from cold workmoderate severity | Use in a cold-worked or unannealed condition where maximum dimensional stability is neededSpecial Metals says the annealed condition should be used where maximum dimensional stability is required. The bulletin gives no drift figure. |
| Sulphur pick-up during hot workinglow severity | Prolonged soaking in the furnace atmosphere before or during forgingHigh Temp Metals advises avoiding prolonged soaking to prevent sulphur absorption from the furnace atmosphere. The page gives no sulphur content or embrittlement data. |
Handling and storage
- Machine in the annealed condition with high speed steel or tungsten carbide tipped tools, using straight cutting oil or soluble oil (Special Metals).
- For welding alloy 42 tooling for aerospace composites, Special Metals introduced NILO Filler Metals CF42. MIG spray and submerged arc welding are not recommended for the NILO series (Special Metals).
- High Temp Metals gives a forging temperature of 2150/2200 °F (1177/1204 °C) and advises avoiding prolonged soaking to prevent sulphur absorption from the furnace atmosphere.
Mitigations
- Anneal at 850 to 1000 °C in a protective atmosphere, the range Special Metals gives for NILO alloys 42 and 48, and use the annealed condition where dimensions must stay fixed.
Supply and geography
How common the raw materials are and where they come from.
Nickel
- Top producers (2025)
- Indonesia 66.7%, Philippines 6.9%, Russia 5.1%, Canada 3.6%
- Recycling
- USGS: nickel recovered from scrap accounted for approximately 60% of apparent consumption in 2025.
- Substitutes
- USGS: titanium alloys can substitute for nickel or nickel-base alloys in corrosive environments.
Documents
Datasheets, safety data sheets, papers and standards you can open.
| Document | Type | Year |
|---|---|---|
| Special Metals: The NILO and NILOMAG Nickel-Iron Alloys (publication SMC-031, Sept 2004) | datasheet | 2004 |
| NeoNickel: Alloy 42 product page (UNS K94100) | datasheet | 2026 |
| Aircraft Materials: Nickel Iron Alloy 42 / Nilo 42 (ASTM F30) technical data sheet | datasheet | 2013 |
| High Temp Metals: Alloy 42 technical data | datasheet | 2015 |
| Studer: 1.3917 Alloy 42/FeNi42 / Ni42 / F1684 / K94100 (product page) | datasheet | 2026 |
| PubChem: Nickel (CID 935), GHS classification summary | database | 2026 |
| USGS Mineral Commodity Summaries 2026, Nickel | report | 2026 |
| METALCOR: Alloy 42 (1.3917), K94100 datasheet | datasheet |
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: alloy-42
spore_version: 0.2
family: nickel-alloys
name: Alloy 42
abbreviation: FeNi42
role: controlled-expansion alloy for glass and ceramic seals
category: metals
type: nickel-superalloys
summary: |
Alloy 42 is a binary nickel-iron alloy with 42 % nickel (UNS K94100, Werkstoff Nr. 1.3917), used where a low, nearly constant thermal expansion is needed up to about 300 °C. Special Metals gives a density of 8.11 g/cm3 and a mean linear expansion of 5.3 ppm/K from 20 to 300 °C, while NeoNickel prints 4.0 to 4.7 ppm/K from 30 to 300 °C. The two suppliers disagree, so both figures are kept. Annealed bar has a tensile strength of 490 MPa and a yield strength of 250 MPa at 20 °C in the Special Metals table.
best_for: Glass-to-metal and ceramic-to-metal seals, and lead frames for integrated circuits, where expansion must stay low up to 300 °C
weakest_at: 'Strength and corrosion data: no corrosion test was found, and the sources disagree on yield strength, tensile strength and elongation'
identity:
formula: 'Fe-42Ni, nominal: a binary nickel-iron alloy with 41 % nickel minimum (42 % nominal) and iron as the balance; carbon 0.05 % maximum, manganese 0.8 % maximum, silicon 0.03 % maximum, chromium 0.25 % maximum, phosphorus and sulphur 0.025 % maximum, aluminium 0.1 % maximum (NeoNickel chemical analysis)'
source: nilo-smc031
where: 'Table 1 (Nominal compositions, NILO alloy 42: Ni 42.0, Fe 58.0) and the opening description (''a binary nickel-iron alloy containing 42% nickel''); maximum limits from the NeoNickel chemical analysis table'
designations:
- system: UNS
code: K94100
source: nilo-smc031
where: Specifications and designations, NILO alloy 42 (UNS K94100, W.Nr. 1.3917)
- system: EN
code: '1.3917'
source: nilo-smc031
where: Specifications and designations, NILO alloy 42 (UNS K94100, W.Nr. 1.3917)
- system: ASTM
code: F30
note: sheet, strip, rod, bar, tubing and wire
source: nilo-smc031
where: Specifications and designations, ASTM F 30 row
- system: ASTM
code: F29
note: wire
source: nilo-smc031
where: Specifications and designations, ASTM F 29 (Wire) row
- system: ASTM
code: B753
note: sheet and strip
source: nilo-smc031
where: Specifications and designations, ASTM B 753 (Sheet and strip) row
- system: DIN
code: '17745'
source: nilo-smc031
where: Specifications and designations, DIN 17745 (Composition) row
- system: AFNOR
code: NF A54-301
note: composition
source: nilo-smc031
where: Specifications and designations, AFNOR NF A54-301 (Composition) row
- system: ASTM
code: F1684
note: specification named by NeoNickel
source: studer-alloy42
where: Page title, 1.3917 - Alloy 42/FeNi42 / Ni42 / F1684 / K94100
- system: Trade name
code: Nilo 42
source: aircraftmaterials-al42
where: Specifications list, Tradename Nilo 42
tags:
environments: []
stresses:
- extreme-cold
applications:
- electronics-and-chips
- cryogenic-fuel
- mechanisms
- structures
properties:
- benchmark: density
label: Density, NILO alloy 42 (Special Metals)
value: 8.11
unit: g/cm3
scope: material
conditions:
temperature: not stated in Table 2
unit_in_source: 0.293 lb/in3
method: Value printed in a Special Metals technical bulletin (publication SMC-031, Sept 2004)
status: ground
source: nilo-smc031
where: Table 2 (Density), row NILO alloy 42
- benchmark: density
label: Density, Alloy 42 (NeoNickel)
value: 8.12
unit: g/cm3
scope: material
conditions:
temperature: not stated
method: Value printed in a stockist product page (NeoNickel)
status: ground
note: Differs from the 8.11 g/cm3 printed by Special Metals; both are kept.
source: neonickel-alloy42
where: Key Properties, row Density
- benchmark: melting_point
label: Melting range, Alloy 42 (NeoNickel)
value: 1425
value_high: 1435
bound: range
unit: °C
scope: material
conditions:
basis: melting range as printed
unit_in_source: 1425°C - 1435°C
method: Range printed in a stockist product page (NeoNickel)
status: ground
source: neonickel-alloy42
where: Key Properties, row Melting Range
- benchmark: melting_point
label: Melting point, NILO alloy 42 (Special Metals)
value: 1435
unit: °C
scope: material
conditions:
unit_in_source: 2615 °F
method: Value printed in a Special Metals technical bulletin, Table 3
status: ground
note: Special Metals gives a single figure at the top of the NeoNickel range.
source: nilo-smc031
where: Table 3 (Melting and Inflection Points), row NILO alloy 42
- benchmark: melting_point
label: Melting point, Alloy 42 (High Temp Metals)
value: 1427
unit: °C
scope: material
conditions:
unit_in_source: 2600 °F
method: Value printed in a supplier technical data sheet
status: ground
source: hightemp-alloy42
where: Physical Properties table, row Melting Point, °C column
- benchmark: curie_temperature
label: Curie temperature, Alloy 42 (NeoNickel)
value: 380
unit: °C
scope: material
conditions:
basis: as printed on the product page; no test method given
method: Value printed in a stockist product page (NeoNickel)
status: ground
note: High Temp Metals prints the same 380 °C (715 °F).
source: neonickel-alloy42
where: Key Properties, row Curie Temperature
- benchmark: thermal_conductivity
label: Thermal conductivity, NILO alloy 42 (Special Metals)
value: 10.5
unit: W/m°C
scope: material
conditions:
temperature: 20 °C (68 °F)
unit_in_source: W/m°C; 72.8 Btu in/ft2h °F
method: Value printed in a Special Metals technical bulletin, Table 4
status: ground
source: nilo-smc031
where: Table 4 (Thermal Conductivity at 20 °C), row NILO alloy 42
- benchmark: thermal_conductivity
label: Thermal conductivity, Alloy 42 (NeoNickel)
value: 10.7
unit: W/m-K
scope: material
conditions:
temperature: 20/100 °C, as printed
method: Value printed in a stockist product page (NeoNickel)
status: ground
note: Special Metals gives 10.5 W/m°C at 20 °C; High Temp Metals prints 10.7 W/m-K at 20/100 °C too.
source: neonickel-alloy42
where: Key Properties, row Thermal Conductivity at 20/100°C
- benchmark: cte
label: Mean linear expansion, 20 to 300 °C, typical (Special Metals)
value: 5.3
unit: ppm/K
scope: material
conditions:
temperature_range: 20 to 300 °C (68 to 572 °F)
basis: typical mean linear coefficient for NILO alloy 42 as printed
unit_in_source: 10-6/°C
method: Typical value printed in a Special Metals technical bulletin, Table 8 (not a guaranteed minimum or maximum)
status: ground
note: Differs from the 4.0 to 4.7 ppm/K printed by NeoNickel and High Temp Metals for 30 to 300 °C; both are kept and the sources are not reconciled.
source: nilo-smc031
where: Table 8 (Typical Thermal Expansion of NILO alloy 42), row 20-300
- benchmark: cte
label: Mean linear expansion, 30 to 300 °C (NeoNickel)
value: 4
value_high: 4.7
bound: range
unit: ppm/K
scope: material
conditions:
temperature_range: 30 to 300 °C
unit_in_source: 10-6/°C
method: Range printed on a stockist product page (NeoNickel); High Temp Metals prints the same range
status: ground
source: neonickel-alloy42
where: Key Properties, Coefficient of Thermal Expansion, row 30 to 300°C
- benchmark: cte
label: Mean linear expansion, 30 to 450 °C (NeoNickel)
value: 6.7
value_high: 7.4
bound: range
unit: ppm/K
scope: material
conditions:
temperature_range: 30 to 450 °C
unit_in_source: 10-6/°C
method: Range printed on a stockist product page (NeoNickel)
status: ground
source: neonickel-alloy42
where: Key Properties, Coefficient of Thermal Expansion, row 30 to 450°C
- benchmark: elastic_modulus
label: Elastic modulus, NILO alloy 42 (Special Metals)
value: 150
unit: GPa
scope: material
conditions:
temperature: not stated in Table 16
unit_in_source: 21.8 x 10^3 ksi
method: Value printed in a Special Metals technical bulletin, Table 16
status: ground
source: nilo-smc031
where: Table 16 (Elastic Modulus Data), row NILO alloy 42
- benchmark: elastic_modulus
label: Elastic modulus at 20 °C, Alloy 42 (NeoNickel)
value: 148
unit: GPa
scope: material
conditions:
temperature: 20 °C
method: Value printed in a stockist product page (NeoNickel)
status: ground
source: neonickel-alloy42
where: Key Properties, row Modulus of Elasticity at 20°C
- benchmark: yield_strength
label: Yield strength (0.2% offset), annealed bar at 20 °C (Special Metals)
value: 250
unit: MPa
scope: material
conditions:
temper: annealed, hot-rolled bar
temperature: 20 °C (68 °F)
test: 0.2% offset
unit_in_source: 36.0 ksi
method: Value printed in a Special Metals technical bulletin, Table 12
status: ground
source: nilo-smc031
where: Table 12 (Typical Mechanical Properties of NILO alloy 42), 20 °C row
- benchmark: yield_strength
label: Yield strength (0.2% offset), annealed at room temperature (Aircraft Materials)
value: 250
unit: MPa
scope: material
conditions:
temper: annealed
test: 0.2% offset
unit_in_source: 36,000 psi
method: Value printed in a supplier technical data sheet (Typical Mechanical Properties table)
status: ground
source: aircraftmaterials-al42
where: Typical Mechanical Properties table, row Alloy 42 (Nilo 42), annealed
- benchmark: ultimate_tensile_strength
label: Tensile strength, annealed bar at 20 °C (Special Metals)
value: 490
unit: MPa
scope: material
conditions:
temper: annealed, hot-rolled bar
temperature: 20 °C (68 °F)
unit_in_source: 71.0 ksi
method: Value printed in a Special Metals technical bulletin, Table 12
status: ground
note: The same 490 MPa is printed by Aircraft Materials for annealed material; High Temp Metals prints 517 MPa.
source: nilo-smc031
where: Table 12 (Typical Mechanical Properties of NILO alloy 42), 20 °C row
- benchmark: ultimate_tensile_strength
label: Tensile strength, annealed material (High Temp Metals)
value: 517
unit: MPa
scope: material
conditions:
temper: annealed, material as tested by the supplier
unit_in_source: 75 ksi
method: Typical value printed in a supplier technical data sheet
status: ground
note: Differs from the 490 MPa printed by Special Metals and Aircraft Materials; both are kept.
source: hightemp-alloy42
where: Typical Mechanical Properties table, annealed row
- benchmark: elongation
label: Elongation on 50 mm (2 in), annealed bar at 20 °C (Special Metals)
value: 43
unit: '%'
scope: material
conditions:
temper: annealed, hot-rolled bar
temperature: 20 °C (68 °F)
gauge: 50 mm (2 inch)
method: Value printed in a Special Metals technical bulletin, Table 12
status: ground
source: nilo-smc031
where: Table 12 (Typical Mechanical Properties of NILO alloy 42), 20 °C row, elongation column
- benchmark: elongation
label: Elongation in 2 in, annealed (High Temp Metals)
value: 30
unit: '%'
scope: material
conditions:
temper: annealed
gauge: 2 in
method: Typical value printed in a supplier technical data sheet
status: ground
note: Differs from the 43 % printed by Special Metals; both are kept.
source: hightemp-alloy42
where: Typical Mechanical Properties table, annealed row, % Elongation in 2 in column
- benchmark: electrical_resistivity
label: Electrical resistivity at 20 °C, NILO alloy 42 (Special Metals)
value: 61
unit: microhm-cm
scope: material
conditions:
temperature: 20 °C (68 °F)
unit_in_source: 61 microhm cm (367 ohm circ mil/ft)
method: Value printed in a Special Metals technical bulletin, Table 6
status: ground
source: nilo-smc031
where: Table 6 (Electrical Resistivity), row 20 °C, NILO alloy 42 column
- benchmark: electrical_resistivity
label: Electrical resistivity, Alloy 42 (High Temp Metals)
value: 66
unit: microhm-cm
scope: material
conditions:
temperature: not stated
unit_in_source: 400 ohm-cir mil/ft
method: Value printed in a supplier technical data sheet
status: ground
note: Differs from the 61 microhm-cm at 20 °C printed by Special Metals; both are kept.
source: hightemp-alloy42
where: Physical Properties table, row Electrical resistivity
- benchmark: specific_heat
label: Specific heat, Alloy 42 (High Temp Metals)
value: 0.5
unit: kJ/kg-K
scope: material
conditions:
temperature: not stated
unit_in_source: 0.12 Btu/lb-°F
method: Value printed in a supplier technical data sheet
status: ground
source: hightemp-alloy42
where: Physical Properties table, row Specific heat
- benchmark: density
label: Density, 1.3917 Alloy 42 (METALCOR)
value: 8.15
unit: g/cm3
scope: material
conditions:
temperature: 20 °C
method: Value printed in a METALCOR datasheet, Physical Properties 20°C table
status: ground
note: Third density figure for this alloy; Special Metals gives 8.11 g/cm3 and NeoNickel 8.12 g/cm3. All three are kept.
source: metalcor-alloy42
where: Physical Properties 20°C table, row Density
- benchmark: thermal_conductivity
label: Thermal conductivity, 1.3917 Alloy 42 (METALCOR)
value: 12.5
unit: W/m K
scope: material
conditions:
temperature: 20 °C
method: Value printed in a METALCOR datasheet, Physical Properties 20°C table
status: ground
note: Higher than the 10.5 W/m°C (Special Metals) and 10.7 W/m-K (NeoNickel) figures. All three are kept and not reconciled.
source: metalcor-alloy42
where: Physical Properties 20°C table, row Thermal conductivity
- benchmark: yield_strength
label: Yield strength Rp (0.2% proof), lower limit at 20 °C (METALCOR)
value: 300
bound: lower
unit: N/mm2
scope: material
conditions:
temperature: 20 °C
test: 0.2% proof (Rp) as printed
basis: lower limit printed with the sign ≥
method: Lower limit printed in a METALCOR datasheet, Mechanical Properties 20°C table
status: ground
note: A lower limit, not a typical value, so it is not directly comparable with the 250 MPa typical yield from Special Metals. Both are kept.
source: metalcor-alloy42
where: Mechanical Properties 20°C table, row 0.2% yield strength Rp
- benchmark: ultimate_tensile_strength
label: Tensile strength Rm, lower limit at 20 °C (METALCOR)
value: 500
bound: lower
unit: N/mm2
scope: material
conditions:
temperature: 20 °C
basis: lower limit printed with the sign ≥
method: Lower limit printed in a METALCOR datasheet, Mechanical Properties 20°C table
status: ground
note: A lower limit, not a typical value. Special Metals prints 490 MPa typical and High Temp Metals 517 MPa; all are kept.
source: metalcor-alloy42
where: Mechanical Properties 20°C table, row Tensile strength Rm
- benchmark: elastic_modulus
label: Modulus of elasticity, 1.3917 Alloy 42 (METALCOR)
value: 145
unit: kN/mm2
scope: material
conditions:
temperature: 20 °C
method: Value printed in a METALCOR datasheet, Mechanical Properties 20°C table
status: ground
note: Lower than the 148 GPa (NeoNickel) and 150 GPa (Special Metals) figures. All three are kept.
source: metalcor-alloy42
where: Mechanical Properties 20°C table, row Modulus of elasticity
corrosion:
- environment: Air under standard service conditions
headline: The supplier describes Alloy 42 as strongly resistant to oxidation and corrosion, with no test data given.
effect: Studer describes the alloy as having strong resistance to oxidation and corrosion under standard service conditions. The page names no environment, exposure time, test standard or corrosion rate.
rating: low
conditions:
basis: qualitative supplier statement; standard service conditions not defined
test: none stated
method: Qualitative statement read from the supplier product page
source: studer-alloy42
where: Description text, 1.3917 Alloy 42 page
- environment: Annealing atmosphere at 850 to 1000 °C
headline: Alloy 42 is annealed at 850 to 1000 °C in a protective atmosphere, and the bulletin gives no oxidation rate.
effect: Special Metals says that NILO alloys 42 and 48 can be annealed at 850 to 1000 °C in a protective atmosphere. The bulletin does not give an oxide thickness, a scaling rate or the type of protective gas.
rating: unknown
conditions:
temperature_range: 850 to 1000 °C (1560 to 1830 °F)
atmosphere: protective atmosphere, type not named
method: Heat-treatment instruction printed in a Special Metals technical bulletin
source: nilo-smc031
where: Heat Treatment, section NILO alloys 42 and 48
risks:
hazards:
- text: PubChem's GHS summary for nickel (CID 935) lists H317, 'May cause an allergic skin reaction', H351, 'Suspected of causing cancer', and H412, 'Harmful to aquatic life with long lasting effects'. Alloy 42 is 41 % nickel minimum, so these are the hazard data we hold for it.
ghs:
- H317
- H351
- H412
source: pubchem-nickel
where: Safety and Hazards, GHS Classification summary lines (CID 935, Nickel)
failure_risks:
- mode: Dimensional drift from cold work
trigger: Use in a cold-worked or unannealed condition where maximum dimensional stability is needed
consequence: Special Metals says the annealed condition should be used where maximum dimensional stability is required. The bulletin gives no drift figure.
severity: moderate
source: nilo-smc031
where: Heat Treatment, section NILO alloys 42 and 48
- mode: Sulphur pick-up during hot working
trigger: Prolonged soaking in the furnace atmosphere before or during forging
consequence: High Temp Metals advises avoiding prolonged soaking to prevent sulphur absorption from the furnace atmosphere. The page gives no sulphur content or embrittlement data.
severity: low
source: hightemp-alloy42
where: Workability, Forging
side_effects: []
handling:
- text: Machine in the annealed condition with high speed steel or tungsten carbide tipped tools, using straight cutting oil or soluble oil (Special Metals).
source: nilo-smc031
where: Machining section
- text: For welding alloy 42 tooling for aerospace composites, Special Metals introduced NILO Filler Metals CF42. MIG spray and submerged arc welding are not recommended for the NILO series (Special Metals).
source: nilo-smc031
where: Fabrication section
- text: High Temp Metals gives a forging temperature of 2150/2200 °F (1177/1204 °C) and advises avoiding prolonged soaking to prevent sulphur absorption from the furnace atmosphere.
source: hightemp-alloy42
where: Workability, Forging
mitigations:
- text: Anneal at 850 to 1000 °C in a protective atmosphere, the range Special Metals gives for NILO alloys 42 and 48, and use the annealed condition where dimensions must stay fixed.
source: nilo-smc031
where: Heat Treatment, section NILO alloys 42 and 48
uses:
- application: electronics-and-chips
device: Semiconductor lead frames in integrated circuits
example: Aircraft Materials says Alloy 42 (Nilo 42) is used for semiconductor lead frames in integrated circuits.
source: aircraftmaterials-al42
where: Introduction paragraph
- application: electronics-and-chips
device: Glass-to-metal seals in electronic tubes and lamps
example: High Temp Metals says Alloy 42 has been used for the glass-to-metal seals in electronic tubes, automotive and industrial lamps, transformer and capacitor bushings.
source: hightemp-alloy42
where: Applications
- application: structures
device: Tooling for aerospace composites
example: Special Metals says NILO alloy 42 is used for tooling for aerospace composites and for thermostat rods.
source: nilo-smc031
where: Introduction (page 1, description of NILO alloy 42)
- application: cryogenic-fuel
device: Cryogenic components and liquid-gas storage tanks
example: NeoNickel lists cryogenic components among the applications of Alloy 42, and says it shows low thermal expansion from cryogenic temperatures up to 300 °C.
source: neonickel-alloy42
where: Characteristics and Applications of Alloy 42
- application: mechanisms
device: Thermostatic bimetal strip
example: Special Metals says NILO alloy 42 is used in thermostatic bi-metal strip, as the low-expansion component.
source: nilo-smc031
where: Introduction (page 1, description of NILO alloy 42)
- application: cryogenic-fuel
device: Tanks for liquid natural gas
example: METALCOR lists tanks for liquid natural gas, with measuring and thermostatic instruments, among the applications of 1.3917 Alloy 42.
source: metalcor-alloy42
where: Application row
supply:
- subject: Nickel
producers:
- country: Indonesia
share_percent: 66.7
year: 2025
- country: Philippines
share_percent: 6.9
year: 2025
- country: Russia
share_percent: 5.1
year: 2025
- country: Canada
share_percent: 3.6
year: 2025
critical_lists: []
recycling: 'USGS: nickel recovered from scrap accounted for approximately 60% of apparent consumption in 2025.'
substitutes:
- 'USGS: titanium alloys can substitute for nickel or nickel-base alloys in corrosive environments.'
source: usgs-mcs2026-nickel
where: World Mine Production and Reserves table, mine production 2025e (world total 3,900,000 t, nickel content; shares calculated by Space Mushroom from the printed country values 2,600,000, 270,000, 200,000 and 140,000 t, method approximate); Recycling; Substitutes. Critical-list status not read in this run.
media: []
documents:
- title: 'Special Metals: The NILO and NILOMAG Nickel-Iron Alloys (publication SMC-031, Sept 2004)'
type: datasheet
url: https://www.specialmetals.com/documents/technical-bulletins/nilo-alloys.pdf
year: 2004
- title: 'NeoNickel: Alloy 42 product page (UNS K94100)'
type: datasheet
url: https://www.neonickel.com/alloys/all-alloys/alloy-42
year: 2026
- title: 'Aircraft Materials: Nickel Iron Alloy 42 / Nilo 42 (ASTM F30) technical data sheet'
type: datasheet
url: https://aircraftmaterials.com/data/nickel/al42.html
year: 2013
- title: 'High Temp Metals: Alloy 42 technical data'
type: datasheet
url: https://hightempmetals.com/techdata/hitempInvar42data.php
year: 2015
- title: 'Studer: 1.3917 Alloy 42/FeNi42 / Ni42 / F1684 / K94100 (product page)'
type: datasheet
url: https://www.studersa.com/en/materials/13917-alloy-42-feni42-ni42-f1684-k94100;138
year: 2026
- title: 'PubChem: Nickel (CID 935), GHS classification summary'
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/935
year: 2026
- title: USGS Mineral Commodity Summaries 2026, Nickel
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-nickel.pdf
year: 2026
- title: 'METALCOR: Alloy 42 (1.3917), K94100 datasheet'
type: datasheet
url: http://www.metalcor.de/en/datenblatt/80/
gaps:
- No flight, vacuum, radiation or thermal-vacuum result for Alloy 42 was found. The two NASA reports searched (NTRS 19740012950 and 19680006647) name Kovar but not Alloy 42.
- No corrosion test (salt spray, humid air, immersion, or oxidation rate) was found. The only corrosion statement is a qualitative supplier phrase, and no published paper on Alloy 42 oxidation was found.
- No safety data sheet for Alloy 42 itself was read. The hazard data are PubChem's record for elemental nickel.
- Density, melting point, thermal conductivity, elongation and resistivity differ between sources; every figure is kept with its source. The METALCOR datasheet adds a third density (8.15 g/cm3) and conductivity (12.5 W/m K), and its strength values are lower limits. Special Metals and NeoNickel disagree on the expansion figures at 20 to 300 °C (5.3 against 4.0 to 4.7 ppm/K).
- DIN 17744 is printed by NeoNickel but DIN 17745 by Special Metals and Aircraft Materials. Only DIN 17745 is listed.
- Hardness (Special Metals Table 15, annealed 76 Rockwell B maximum) is not recorded because its benchmark name is not in the canonical list.
- Nickel's status on the USGS 2025 critical minerals list and the EU critical raw materials list was not read in this run, so critical_lists is empty.
- Iron supply was not read. Only nickel supply is given.
- Welding filler and weld-metal property data beyond the CF42 filler name were not found.
sources:
nilo-smc031:
title: The NILO and NILOMAG Nickel-Iron Alloys (Special Metals Corporation, publication SMC-031)
id: Special Metals SMC-031, copyright 2004 (Sept 04)
url: https://www.specialmetals.com/documents/technical-bulletins/nilo-alloys.pdf
year: 2004
kind: datasheet
license: manufacturer document, linked not reproduced
neonickel-alloy42:
title: Alloy 42, NeoNickel product page (Key Properties, Chemical analysis, Characteristics)
id: NeoNickel, Alloy 42 page; UNS K94100
url: https://www.neonickel.com/alloys/all-alloys/alloy-42
year: 2026
kind: web
license: stockist web page, cited not reproduced
aircraftmaterials-al42:
title: Nickel Iron Alloy 42 / Nilo 42 (ASTM F30), Technical Data Sheet (Aircraft Materials)
id: Aircraft Materials, UNS K94100
url: https://aircraftmaterials.com/data/nickel/al42.html
year: 2013
kind: datasheet
license: supplier document, cited not reproduced
hightemp-alloy42:
title: Alloy 42 Technical Data (High Temp Metals)
id: High Temp Metals, Alloy 42 technical data page
url: https://hightempmetals.com/techdata/hitempInvar42data.php
year: 2015
kind: datasheet
license: supplier document, cited not reproduced
studer-alloy42:
title: 1.3917 - Alloy 42/FeNi42 / Ni42 / F1684 / K94100 (Studer SA, product page)
id: Studer, Werkstoffe 1.3917
url: https://www.studersa.com/en/materials/13917-alloy-42-feni42-ni42-f1684-k94100;138
year: 2026
kind: web
license: stockist web page, cited not reproduced
pubchem-nickel:
title: PubChem compound record, Nickel (CID 935), GHS classification
id: CID 935
url: https://pubchem.ncbi.nlm.nih.gov/compound/935
year: 2026
kind: database
license: public domain (NCBI)
usgs-mcs2026-nickel:
title: Mineral Commodity Summaries 2026, Nickel
id: USGS MCS 2026, February 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-nickel.pdf
year: 2026
kind: report
license: public domain (USGS)
metalcor-alloy42:
title: Alloy 42 (1.3917), K94100 datasheet (METALCOR)
id: METALCOR datasheet 80, Alloy 42
url: http://www.metalcor.de/en/datenblatt/80/
kind: datasheet
license: supplier document, cited not reproduced
license: CC-BY-4.0
updated: '2026-11-01'
review:
status: draft
method: assistant
checked_values: 27
unreachable: 0
caveats: 3
note: Read by an AI assistant on 2026-11-01. Values were read from fetched pages (Special Metals PDF, NeoNickel, Aircraft Materials, High Temp Metals, Studer). Where sources disagree, both values are kept and noted.
story:
recipe:
line: Alloy 42 is a binary nickel-iron alloy. It is about 42 % nickel with iron as the balance, plus small maximum limits on carbon, manganese, silicon, chromium, phosphorus, sulphur and aluminium (Special Metals; NeoNickel).
parts:
- name: Nickel
symbol: Ni
share_percent: 41
role: 41 % minimum in the chemical limits; the nominal 42 % gives the alloy its name (NeoNickel; Special Metals Table 1).
- name: Iron
symbol: Fe
role: The balance of the composition in every limit table read.
- name: Carbon
symbol: C
share_high: 0.05
role: Maximum 0.05 % (Aircraft Materials; High Temp Metals).
- name: Manganese
symbol: Mn
share_high: 0.8
role: Maximum 0.8 % (NeoNickel).
- name: Silicon
symbol: Si
share_high: 0.03
role: Maximum 0.03 % (NeoNickel).
- name: Chromium
symbol: Cr
share_high: 0.25
role: Maximum 0.25 % (NeoNickel).
- name: Phosphorus
symbol: P
share_high: 0.025
role: Maximum 0.025 % (NeoNickel).
- name: Sulphur
symbol: S
share_high: 0.025
role: Maximum 0.025 % (NeoNickel).
- name: Aluminium
symbol: Al
share_high: 0.1
role: Maximum 0.1 % (NeoNickel).
risk_groups:
- title: For people
level: 0
verdict: 'Nickel content: skin sensitiser, suspected carcinogen'
lead: No safety data sheet for Alloy 42 itself was read. The hazard data we hold are PubChem's record for nickel, and Alloy 42 is 41 % nickel minimum.
points:
- label: The nickel record
line: PubChem's nickel summary lists skin sensitisation, suspected cancer and harm to aquatic life. These are hazards of the element, not a test of the alloy.
- label: Dust and fume
line: Machining, grinding and welding make metal dust and fume. Handle the material as a nickel-containing alloy and avoid breathing the dust.
- title: If the alloy is heated
verdict: Hot working needs a controlled furnace atmosphere
lead: These instructions come from the suppliers' heat-treatment and forging advice, not from incident reports.
points:
- label: Annealing
line: Special Metals gives an annealing range of 850 to 1000 °C in a protective atmosphere for NILO alloys 42 and 48.
- label: Forging
line: High Temp Metals advises a forging temperature of 2150/2200 °F and avoiding prolonged soaking, which can pick up sulphur from the furnace atmosphere.
- title: Handling and fabrication
verdict: Machine annealed; weld with the matching filler
lead: The fabrication advice below comes from the Special Metals bulletin and the High Temp Metals data sheet.
points:
- label: Machining
line: Machine in the annealed condition with high speed steel or tungsten carbide tipped tools.
- label: Welding
line: For tooling welds, Special Metals introduced NILO Filler Metals CF42. MIG spray and submerged arc welding are not recommended for the NILO series.
why: Alloy 42 is a nickel-iron alloy with about 42 % nickel. Its thermal expansion is low and nearly constant from room temperature to about 300 °C, which is why it is used where it must seal to glass or ceramic, or hold a dimension while the temperature changes. The sources name lead frames in integrated circuits, glass-to-metal seals in electronic tubes and lamps, and tooling that shapes aerospace composites as its uses.
uses:
- where: Electronic packages
line: Aircraft Materials says Alloy 42 is used for semiconductor lead frames in integrated circuits. High Temp Metals says it has been used for glass-to-metal seals in electronic tubes and lamps.
- where: Composite tooling
line: Special Metals says NILO alloy 42 is used for tooling for aerospace composites, and NeoNickel lists composite tooling among its applications.
- where: Cryogenic and bimetal parts
line: NeoNickel lists cryogenic components and liquid-gas storage tanks. Special Metals lists its use in thermostatic bi-metal strip as the low-expansion component.
can_do:
- label: Low expansion
value: 4.0 to 4.7 ppm/K
benchmark: cte
line: Holds a low, nearly constant expansion from cryogenic temperatures up to about 300 °C (NeoNickel), and NeoNickel prints a mean of 4.0 to 4.7 ppm/K from 30 to 300 °C.
- label: Strength when annealed
value: 490 MPa tensile, 250 MPa yield
benchmark: ultimate_tensile_strength
line: Annealed bar has a tensile strength of 490 MPa and a yield strength of 250 MPa at 20 °C (Special Metals Table 12).
- label: Stiffness
value: 150 GPa
benchmark: elastic_modulus
line: Elastic modulus of 150 GPa (Special Metals Table 16), against 148 GPa at 20 °C on the NeoNickel page.
compare: Alloy 42 has a density of 8.11 g/cm3 in Special Metals' table and 8.12 g/cm3 in NeoNickel's, so the two sources differ only slightly. On expansion, Special Metals' typical table gives a mean linear coefficient of 5.3 ppm/K from 20 to 300 °C, while NeoNickel gives 4.0 to 4.7 ppm/K from 30 to 300 °C. The sources disagree on this figure, so the conditions of each value matter more than the single number. The table compares the three properties most often used to choose the alloy.
compare_rows:
- label: Density
benchmark: density
- label: Thermal expansion
benchmark: cte
- label: Thermal conductivity
benchmark: thermal_conductivity
handling:
- Machine in the annealed condition, with high speed steel or tungsten carbide tipped tools.
- Use NILO Filler Metals CF42 for tooling welds, and avoid MIG spray and submerged arc welding.
- Anneal at 850 to 1000 °C in a protective atmosphere.
- Avoid prolonged soaking in the furnace to prevent sulphur pick-up.
good_for:
- 'Low expansion to about 300 °C: 4.0 to 4.7 ppm/K from 30 to 300 °C (NeoNickel), for glass and ceramic seals.'
- Lead frames and bimetal parts, where the alloy is named in both the Aircraft Materials and Special Metals sources.
watch_out:
- The sources disagree on expansion (5.3 against 4.0 to 4.7 ppm/K), on tensile strength (490 against 517 MPa) and on elongation (43 against 30 %).
- No corrosion test data were found, and the only corrosion statement is a qualitative supplier phrase.
- Alloy 42 is a nickel alloy, so its hazard data come from the nickel record.
verdict: Alloy 42 is a low-expansion nickel-iron alloy for glass seals, lead frames and composite tooling, with consistent density and modulus data. The expansion figures and strength values differ by source, and no flight or corrosion test data were found.
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.
| # | Source | Type | Year | Used for |
|---|---|---|---|---|
| The NILO and NILOMAG Nickel-Iron Alloys (Special Metals Corporation, publication SMC-031) | datasheet | 2004 | 17 values | |
| Alloy 42, NeoNickel product page (Key Properties, Chemical analysis, Characteristics) | web | 2026 | 8 values | |
| Nickel Iron Alloy 42 / Nilo 42 (ASTM F30), Technical Data Sheet (Aircraft Materials) | datasheet | 2013 | 2 values | |
| Alloy 42 Technical Data (High Temp Metals) | datasheet | 2015 | 8 values | |
| 1.3917 - Alloy 42/FeNi42 / Ni42 / F1684 / K94100 (Studer SA, product page) | web | 2026 | 1 value | |
| PubChem compound record, Nickel (CID 935), GHS classification | database | 2026 | 1 value | |
| Mineral Commodity Summaries 2026, Nickel | report | 2026 | 1 value | |
| Alloy 42 (1.3917), K94100 datasheet (METALCOR) | datasheet | 6 values |
Updated