Silver Ag

Ag · CAS 7440-22-4 · face-centred cubic

Silver is a soft, dense, face-centred cubic metal with the highest electrical conductivity of any metal.

17 sources · Updated 2026-10-17 · CC BY 4.0

Evidence level

5 of 5

Flown or field-proven

Conduct electricity

1.63 µΩ·cm

Conduct heat

429 W/(m K)

Reflect light

About 98% at 400 to 1000 nm

Carry load

172 to 330 MPa

Recipe, share of the weight

  • Ag 100.0%Silver

Best for

Electrical and heat conduction and light reflection (resistivity 1.63 microohm cm, thermal conductivity 429 W/(m K) at 0 to 100 degC)

Weakest at

Unprotected exposure to atomic oxygen in low Earth orbit (black oxide that cracks and spalls) and to sulphur compounds in air (silver sulphide tarnish)

Risk at a glance

  • People Low. Classification depends on the form
  • If it fails High. Silver oxide blackening and flaking in orbit
  • Corrosion Severe. Exposed silver is quickly turned into a black oxide that cracks and flakes off.

Quick facts: Ag

Key properties of Ag
PropertyValueBasis
Density10.5 g/cm³1 sourced value
Thermal conductivity429 W/(m·K)1 sourced value
Thermal expansion (CTE)19.1 ppm/K1 sourced value
Melting point962 °C1 sourced value
Specific heat237 J/(kg·K)1 sourced value
Electrical resistivity1.6e-8 Ω·m1 sourced value

What is the density of Silver (Ag)?

Silver (Ag) has a density of 10.5 g/cm³. The source and test conditions are listed in the properties table on this page.

What is the thermal conductivity of Silver (Ag)?

Silver (Ag) has a thermal conductivity of 429 W/(m·K). The source and test conditions are listed in the properties table on this page.

What is the coefficient of thermal expansion of Silver (Ag)?

Silver (Ag) has a coefficient of thermal expansion of 19.1 ppm/K. The source and test conditions are listed in the properties table on this page.

What is the melting point of Silver (Ag)?

Silver (Ag) has a melting point of 962 °C. The source and test conditions are listed in the properties table on this page.

What is Silver (Ag) used for?

Uses recorded in the sources include Silvered FEP Teflon (second-surface mirror) thermal blankets; Final contact metal on GaAs solar cells and evaporated contacts on thin silicon cells, with silver-plated Invar interconnect tabs; Screen-printed silver ink front contacts for photovoltaic cells (research).

Why it exists

Silver is a soft, dense metal, atomic number 47, with a face-centred cubic crystal structure. Its single outer electron makes it an unusually good conductor: the Goodfellow table gives an electrical resistivity of 1.63 microohm cm at 20 °C and a thermal conductivity of 429 W/(m K) between 0 and 100 °C. Wikipedia, citing a handbook, states that silver has the highest electrical conductivity of all metals. It melts at 961.9 °C and has a density of 10.5 g/cm3. The same properties make it a good mirror, which is why it sits behind the Teflon film in thermal blankets. Its weakness is chemical. Sulphur compounds in air turn it into dark silver sulphide, and atomic oxygen in low Earth orbit turns exposed silver into a black oxide that cracks and flakes away, so spacecraft use almost always buries it under another layer.

Where it's used

Thermal blankets

Silvered FEP Teflon is a second-surface mirror: sunlight passes through the transparent film and is reflected by the silver behind it, while the film radiates heat. The LDEF specimens carried about 1600 angstrom of silver on 5 mil FEP and flew for 5 years and 9 months.

Solar cells

A TRW and JPL study used GaAs cells whose last contact metal was silver, silicon cells with evaporated silver contacts, and silver plated Invar tabs welded as interconnects. A Purdue and JPL study looked at silver inks for printed cell contacts.

Circuit boards

Phone circuit boards contain silver. One study leached whole boards from a single phone model and found 123.35 g of silver per ton of boards, while a Chalmers study measured silver in 30 mobile phones and 30 smartphones.

Mirrors and optics

A silver telescope coating reached an average specular reflectivity of about 98% between 400 and 1000 nm.

Recipe

Ag

Silver is the element Ag, atomic number 47, a single-element metal with cubic close-packed crystals (ccp, space group Fm-3m, WebElements). USGS says silver is mostly obtained as a by-product of lead-zinc, copper and gold mines, and that its polymetallic ore deposits account for more than two-thirds of resources. In 2025, 24 US refiners produced commercial-grade silver from domestic and foreign ores, concentrates and scrap, with about 1,000 tons recovered from new and old scrap (USGS).

What Ag is made of
IngredientAtoms per unitShare of the weightWhat it does
Silver Ag 1 100.0% The whole material. WebElements prints the relative atomic mass on its main page.

Weight shares are calculated from standard atomic weights.

What it can do

Conduct electricity

1.63 µΩ·cm

measured

The Goodfellow bar (99.95% purity) has a resistivity of 1.63 microohm cm at 20 °C with a temperature coefficient of 0.0041 per K.

Conduct heat

429 W/(m K)

measured

Thermal conductivity is 429 W/(m K) over 0 to 100 °C. Heat also makes silver expand by 19.1 ppm/K over the same range.

Reflect light

About 98% at 400 to 1000 nm

A silver-enhanced telescope coating averaged about 98% specular reflectivity from 400 to 1000 nm. This is a protected coating, not bare silver.

Carry load

172 to 330 MPa

Tensile strength is 172 MPa soft and 330 MPa hard, Vickers hardness 25 and 95 kgf/mm2, and tensile modulus 82.7 GPa. Silver is a soft metal and is not used as a structure.

How it compares

No opened source in this record compares silver with other metals on the same test, so no ranking is made here except the Wikipedia statement that silver has the highest electrical conductivity of all metals. Among silver coatings, the sulphur test showed thickness matters: the 86 nm, 130 nm and 200 nm layers gave very low, about 90% and about 97% average reflectivity.

The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.

Benchmarks
MeasurementAgAuPtPdRhRuOsAu alloysAuSnAg 92.5 Cu 7.5Ag alloysPd-AgPd-Cu, Pd-Ni, Pd-CrPt-RhPt-IrPt-W, Pt-Cu
Capacity and energy
Empirical activation energy of silver oxidation by atomic oxygen (early growth)0.1 eV18no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Thermal behavior and safety
Melting point961.9 °C31065 °C1769 °C1555 °C1964 °C2334 °C3033 °C955 °C280 °C788 to 891 °C780 °Cno data1397 °C1840 to 1870 °C1790 to 1800 °C1865 to 1885 °C
Thermal conductivity429 W/(m K)6320 W/(m K)74 W/(m·K)72 W/(m.K)150 W/(m·K)117 W/(m·K)87.6 W/(m·K)49 W/(m K)57 W/mKno data371 W/m K61 W/(m.K)no datano datano datano data
Specific heat237 J/(K kg)8129.1 J/(kg K)132.6 J/(kg·K)no data242.7 J/(kg·K)no data131 J/(kg·K)no datano data245 J K-1 kg-1no datano datano datano datano datano data
Latent heat of fusion103 J/g9no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Physical and electrical
Density at 20 degC10.5 g/cm³119.3 g/cm³21.45 g/cm³12.02 g/cm³12.42 g/cm³12.36 g/cm³22.5 g/cm³15.8 g/cm³14.7 -10.4 g/cm³10 Mg/m310.9 g/cm³10.8 g/cm³19.97 g/cm³21.54 g/cm³21.26 g/cm³
Density at 15 degC (Merck Index, as quoted by PubChem)10.49 g/cm³2no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Electrical resistivity at 20 degC1.63 µΩ·cm52.2×10^-8 ohm m10.6 µΩ·cm10.8 uOhm.cm43.3 nΩ·m71 nΩ·m8.8 µΩ·cm15.5 µΩ·cmno data1.8 µOhmcm20.4 x10-9 ohm m15 uOhm.cmno datano datano data62 to 68 µOhm cm
Vickers hardness, hard condition95 kgf/mm213no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Vickers hardness, soft condition25 kgf/mm214no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Silver layer in silvered FEP Teflon thermal blanket material1600 angstrom17no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Other measurements
Boiling point2212 °C42856 °C3825 °C2963 °C3695 °C4150 °C5012 °Cno datano datano datano datano datano datano datano datano data
Coefficient of thermal expansion19.1 ppm/K714.2 ppm/K8.93 ppm/K11.8 ppm/K8.46 ppm/K6.78 ppm/K4.57 ppm/K14 ppm/K16 ppm/°C19 x10-6 K-119.6 x10-6 per °Cno datano datano datano datano data
Tensile modulus82.7 GPa10no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Tensile strength, hard condition330 MPa11no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Tensile strength, soft condition172 MPa12no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Poisson's ratio0.367 dimensionless150.44 dimensionlessno data0.39 dimensionlessno data0.3 -0.25 -no datano datano datano datano datano datano datano datano data
Designed reflectivity at 500 nm of a 200 nm silver layer in a telescope coating97.85 %16no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Silver in whole mobile-phone circuit boards, aqua regia leach123.3 g/ton of PCB19no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data

Why choose it, and why not

Good for

  • Conduction. A resistivity of 1.63 microohm cm and a thermal conductivity of 429 W/(m K) in the supplier table.
  • Reflection. A protected silver coating averaged about 98% specular reflectivity from 400 to 1000 nm.
  • Solar-cell contacts and interconnects. Silver was the last contact metal on GaAs cells in a TRW and JPL study.

Watch out for

  • Atomic oxygen. Exposed silver forms a black oxide that cracks and spalls, and the Solar Maximum Mission blankets showed flaking.
  • Tarnish. Hydrogen sulphide forms Ag2S, which absorbs visible light and darkens bare silver.
  • Softness and weight. Density is 10.5 g/cm3 and soft silver has a tensile strength of 172 MPa.
  • Supply. Silver is mostly a byproduct of lead-zinc, copper and gold mining, and it was added to the US critical minerals list in 2025.

Silver is the standard choice when conduction or reflection is needed, and spacecraft use it behind covering layers. Flight and ground data agree that bare silver in low Earth orbit oxidises quickly, so a design that exposes it needs protection, and the numeric rates for that attack are still missing from this record.

Technical details

For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.

Cell-level benchmarks

Values for finished cells. These vary by manufacturer, so read the conditions in the notes. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.

Cell-level benchmarks
MeasurementAgAuPtPdRhRuOsAu alloysAuSnAg 92.5 Cu 7.5Ag alloysPd-AgPd-Cu, Pd-Ni, Pd-CrPt-RhPt-IrPt-W, Pt-Cu
Other measurements
Total silver use in a record-low silicon heterojunction solar cell1.4 mg/Wp20no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data

Notes

The method, full conditions and any caveat for the numbered rows above.

Notes for the numbered rows
#MeasurementMethodConditionsCaveat
1Density at 20 degCValue listed in the supplier's online property table (Goodfellow SKU 1000002903)material bar, purity 99.95%temperature 20 °COther density entries exist for silver; see the Merck Index value below.
2Density at 15 degC (Merck Index, as quoted by PubChem)Reference-book value quoted in the PubChem Density sectiontemperature 15 °Ccitation Merck Index, 13th ed., 2001, p. 1525, as listed in the PubChem recordThe same PubChem section also lists 10.5 at 68 degF (NTP, OSHA) and 10.49 for the metal (NIOSH).
3Melting pointValue listed in the supplier's online property tablematerial bar, purity 99.95%—
4Boiling pointValue listed in the supplier's online property tablematerial bar, purity 99.95%—
5Electrical resistivity at 20 degCValue listed in the supplier's online property tablematerial bar, purity 99.95%temperature 20 °CThe same table gives a temperature coefficient of 0.0041 per K over 0 to 100 degC. The Wikipedia infobox lists 15.87 nOhm m (about 1.587 microohm cm) at 20 degC, a slightly lower figure for a purer specimen or a different source, so resistivity varies between references.
6Thermal conductivityValue listed in the supplier's online property tablematerial bar, purity 99.95%temperature 0 to 100 °CThe Wikipedia infobox also lists 429 W/(m K).
7Coefficient of thermal expansionValue listed in the supplier's online property table (written there as x10^-6 per K)material bar, purity 99.95%temperature 0 to 100 °C—
8Specific heatValue listed in the supplier's online property tablematerial bar, purity 99.95%temperature 25 °C—
9Latent heat of fusionValue listed in the supplier's online property tablematerial bar, purity 99.95%The same table gives a latent heat of evaporation of 2390 J/g.
10Tensile modulusValue listed in the supplier's online property tablematerial bar, purity 99.95%condition listed for both hard and soft—
11Tensile strength, hard conditionValue listed in the supplier's online property table (condition read from the table's Hard and Soft columns)material bar, purity 99.95%condition hardThe supplier does not state the test standard or temperature.
12Tensile strength, soft conditionValue listed in the supplier's online property table (condition read from the table's Hard and Soft columns)material bar, purity 99.95%condition softThe supplier does not state the test standard or temperature.
13Vickers hardness, hard conditionValue listed in the supplier's online property tablematerial bar, purity 99.95%condition hard—
14Vickers hardness, soft conditionValue listed in the supplier's online property tablematerial bar, purity 99.95%condition soft—
15Poisson's ratioValue listed in the supplier's online property tablematerial bar, purity 99.95%condition listed for both hard and softThe same table lists a bulk modulus of 103.6 GPa.
16Designed reflectivity at 500 nm of a 200 nm silver layer in a telescope coatingDesigned (optical-model) value listed in the paper's Table 2wavelength 500 nmsilver thickness 200 nmcoating silver with protective and enhancing layers, not bare silverThe paper's abstract reports an average measured specular reflectivity of about 98% from 400 to 1000 nm for the finished enhanced coating. The 86 nm and 130 nm layers gave 97.43% and 97.83% at 500 nm. This is a protected coating design, not bare silver.
17Silver layer in silvered FEP Teflon thermal blanket materialConstruction described in the NASA report (stated as 'approximately 1600A')construction 5 mil FEP Type A Teflon film, vapour-deposited silver on the back, then about 400 angstrom of Inconel, then 3 to 5 mil black urethane-base paint when used as a blanketThe specimens flew on LDEF for 5 years and 9 months.
18Empirical activation energy of silver oxidation by atomic oxygen (early growth)Ellipsometer thickness measurements between exposures, Arrhenius plots; the abstract says 'of the order of 0.1 eV'temperature range 0 to 70 °C in 10 °C stepssample evaporated silver about 10000 angstrom thick on siliconoxygen source plasma asher at 60 W and 800 millitorr, flux estimated at 1e18 per cm2 sThe oxide film thickness grew as the logarithm of exposure time in the early phase. This is a ground plasma test, not a flight rate.
19Silver in whole mobile-phone circuit boards, aqua regia leachSingle characterisation test, reported in the paper's Table 3sample whole circuit boards from mobile phones of one brand and model, about 30 gleach aqua regia, solid to liquid 1 to 20, 2 hours at 60 °Canalysis flame atomic absorptionUncertainty: The paper prints 123.35 in Table 3, 123.85 in the abstract and 123.25 in the conclusions. No repeats are reported.One brand and model only, so it is not an industry average. The Introduction quotes a literature figure of 250 mg silver in the metal fraction and, for mobile phones, 3.5 kg of silver per ton of material (second-hand, from other authors).
20Total silver use in a record-low silicon heterojunction solar cellResult reported in a Fraunhofer ISE press releasecell silicon heterojunctionfront silver-copper pasterear pure copper pasteThe press release says this is about one tenth of the current standard in industrial production and gives 2 mg/Wp as the calculated long-term sustainable target. It does not give the industrial figure.

Corrosion and compatibility

What happens when it meets other materials and environments.

Corrosion and compatibility
EnvironmentConcernWhat happens
Atomic oxygen in low Earth orbit severe Exposed silver is quickly turned into a black oxide that cracks and flakes off.1
Sulphur compounds in air (tarnish) moderate Hydrogen sulphide in air turns silver into dark silver sulphide, which absorbs visible light.2
Atomic-oxygen roughening of silvered FEP Teflon low The Teflon cover is eroded and the blanket goes from mirror-like to frosted, but silver under it is protected until the cover is breached.3
Corrosion details
#EnvironmentDetailsTest conditions
1 Atomic oxygen in low Earth orbit An Auburn University study for NASA states that silver is swiftly attacked by atomic oxygen to form a black oxide layer that subsequently cracks and spalls. On the Solar Maximum Mission, Inconel-protected silver coatings on Teflon showed near total silver reaction and flaking, blackening the strips of tape with a direct view of the orbital environment. On LDEF, silver beneath a micrometeoroid hole in the FEP cover was oxidised to silver oxide in rings around the hole. smm Solar Maximum Mission, about 4 years in orbit, Inconel/silver on FEP Teflonldef 5 years 9 months, 477 km mean altitude (de Rooij gives 335 km at retrieval)lab plasma asher, 0 to 70 °C
2 Sulphur compounds in air (tarnish) A 2022 telescope-coating paper says H2S in air reacts with the silver to form Ag2S, which absorbs visible light and is the main cause of the black tarnish on bare silver. Silver oxides (AgOx) can form by a separate route involving water. In its accelerated sulphur test, a 130 nm silver layer fell to about 82% reflectivity near 500 nm and an 86 nm layer to very low reflectivity near 480 nm, while a 200 nm layer kept an average above 97%. test ZnS heated in vacuum chamber at 5e-3 Pa, 10 min exposure at room temperaturecomparison the paper cites ANSI/EIA-977 as 480 h at 60 °C or 750 h at 105 °C
3 Atomic-oxygen roughening of silvered FEP Teflon Silvered FEP specimens from LDEF changed from specular to diffuse reflectors in step with atomic-oxygen fluence, because atomic oxygen roughened the coating surface. XPS, infrared and thermal analysis found no significant change at the molecular level. exposure 5 years and 9 months on LDEFpositions Row 3 trailing edge stayed specular; Row 9 leading edge turned frosted

Risks and side effects

Hazards to people, what happens when a cell overheats, and how the material is handled and stored.

For people

Solid silver is a low hazard, but the EU classification for bulk silver includes suspected reproductive and repeated-exposure effects, and fine powder is toxic to aquatic life.

Bulk silver
The EU classification quoted by PubChem for silver massive (1 mm or larger) is a warning with H361f (suspected of damaging fertility) and H373 (organ damage through prolonged or repeated exposure).
Powder and nano silver
Silver powder and nano silver add H400 and H410, very toxic to aquatic life, including with long-lasting effects.
Differing notifications
Of the 2,154 company reports in the ECHA aggregate, 28.9% say the substance does not meet GHS hazard criteria, so check the safety data sheet for your supplier and form.

If it fails

These results come from flight exposures of thermal blankets and from laboratory tests, not from failures of a named spacecraft system.

Atomic oxygen
On the Solar Maximum Mission, exposed Inconel-protected silver showed near total silver reaction and flaking, and the strips with a direct view of the environment blackened.
Impacts
On LDEF, a micrometeoroid hole in the FEP cover let atomic oxygen reach the silver, which oxidised in rings around the hole.
Tarnish
In a ground sulphur test, a thin 86 nm silver layer lost most of its reflectivity near 480 nm, while a 200 nm layer kept an average above 97%.

Handling and storage

Safety data sheet
PubChem shows that classification varies by form, so use the data sheet for the specific form, whether bulk, powder or nano.
Storage in air
Sulphur compounds in air tarnish silver, so bare silver parts are kept protected before use.

Test details
The original wording and numbers from the sources, for readers who want them.

Failure risks

Failure risks
FailureTrigger and consequence
Silver oxide blackening and flaking in orbithigh severityDirect exposure of bare or thinly covered silver to atomic oxygen, as on Solar Maximum Mission thermal tapeNear total silver reaction and flaking, with erosion of the Teflon underneath; the reflecting layer is lost.
Oxidation of the silver at micrometeoroid holesmoderate severityA micrometeoroid hole through the FEP cover on LDEFAtomic oxygen reached the silver through the hole and formed rings of silver oxide; the silver layer had locally debonded from the FEP.
Sulphide tarnish before launchmoderate severityHydrogen sulphide in airAg2S forms, absorbs visible light and darkens the surface (observed in a ground test with thin layers losing reflectivity).

Side effects on surrounding parts

Side effects on surrounding parts
AffectsEffect
Coating tests for atomic-oxygen resistanceSilver oxide has a much higher electrical resistance than silver, so oxidation can be followed by the resistance of a thin film. A NASA-related technique uses 250 angstrom silver films as atomic-oxygen sensors under candidate coatings.
Interpretation of the LDEF resultSilicon-containing molecular contamination on silvered FEP from LDEF was discussed as a possible influence on the atomic-oxygen response.

Handling and storage

  • The PubChem record shows hazard classification varies by form; check the safety data sheet for the specific form (bulk, powder or nano) before handling.

Mitigations

  • On spacecraft thermal blankets the silver is placed behind a transparent FEP Teflon film and covered with Inconel, so the silver faces the film and not the space environment.
  • For mirrors, a thicker silver layer (200 nm kept an average reflectivity above 97% after the sulphur test) and protective layers are used; the 130 nm layer averaged about 90%.

Supply and geography

How common the raw materials are and where they come from.

Silver

USGS: silver is primarily obtained as a byproduct from lead-zinc, copper and gold mines; polymetallic deposits account for more than two-thirds of US and world resources. World mine production 25,300 tons in 2024 and an estimated 26,000 tons in 2025. World reserves 610,000 tons.

Top producers (2025)
Mexico 24.2%, Peru 13.8%, China 13.1%, Bolivia 5.8%, Chile 5.4%
Critical mineral lists
US: listed
Recycling
USGS: in 2025 about 1,000 tons of silver was recovered from new and old scrap, about 11% of US apparent consumption. US net import reliance 77% in 2025.
Substitutes
USGS: aluminium and rhodium may replace silver in mirrors and other reflecting surfaces; digital imaging replaces photographic silver; stainless steel and other metals replace silver in some surgical and tableware uses; nonsilver batteries may replace silver batteries in some applications.