Platinum-tungsten and platinum-copper alloys Pt-W, Pt-Cu

Pt-8W: platinum with 8 % tungsten by mass (Pt92/W8). Pt-Cu: carbon-supported PtCux nanoparticles, x = 1.3 by XRF before activation

Also known as PtW8, Hera 158

Platinum-tungsten is a ductile precious-metal alloy.

9 sources · Updated 2026-10-26 · CC BY 4.0

Evidence level

2 of 5

Lab-measured

Density

21.26 g/cm3

Melting

1865 to 1885 °C

Hardness

200 to 300 HV

Catalyst activity

1236 A/g(Pt)

Recipe, share of the weight

  • Pt 92%Platinum
  • W 8%Tungsten

Best for

Fine resistance wire, probes and electrodes that must resist oxidation in air at high temperature (Pt-W), and dealloyed PtCu catalysts in acid electrolyte (Pt-Cu, laboratory).

Weakest at

Density (21.26 g/cm3) and conductivity (2.58 to 2.77 % IACS, a poor conductor). The PtCu catalyst loses much of its copper in acid.

Risk at a glance

  • People Low. Mixed element records
  • If it fails Moderate. Copper loss from the PtCu catalyst surface in acid
  • Corrosion Moderate. Copper leaves the PtCu/C surface during activation in acid, and the copper content falls.

Quick facts: Pt-W, Pt-Cu

Key properties of Pt-W, Pt-Cu
PropertyValueBasis
Density21.3 g/cm³2 sourced values across conditions
Yield strength400 to 1,000 MPa1 sourced value
Tensile strength800 to 1,100 MPa1 sourced value
Young's modulus230 GPa1 sourced value
Melting point1,865 to 1,910 °C2 sourced values across conditions
Electrical resistivity6.2e-7 to 6.8e-7 Ω·m1 sourced value

What is the density of Platinum-tungsten and platinum-copper alloys?

Platinum-tungsten and platinum-copper alloys has a density of 21.3 g/cm³. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What is the melting point of Platinum-tungsten and platinum-copper alloys?

Platinum-tungsten and platinum-copper alloys has a melting point of 1,865 to 1,910 °C. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What is the yield strength of Platinum-tungsten and platinum-copper alloys?

Platinum-tungsten and platinum-copper alloys has a yield strength of 400 to 1,000 MPa. The source and test conditions are listed in the properties table on this page.

What is the tensile strength of Platinum-tungsten and platinum-copper alloys?

Platinum-tungsten and platinum-copper alloys has a tensile strength of 800 to 1,100 MPa. The source and test conditions are listed in the properties table on this page.

What is the Young's modulus of Platinum-tungsten and platinum-copper alloys?

Platinum-tungsten and platinum-copper alloys has a Young's modulus of 230 GPa. The source and test conditions are listed in the properties table on this page.

What are the other names and codes for Platinum-tungsten and platinum-copper alloys?

Platinum-tungsten and platinum-copper alloys is also written as PtW8, Hera 158. Each code is printed in the source listed beside it in the designations table.

What is Platinum-tungsten and platinum-copper alloys used for?

Uses recorded in the sources include Spark plug electrodes; Resistance and heater wire in high-temperature furnaces; Sensor assemblies, microfabricated probe tips and electrical feedthroughs.

Why it exists

Platinum-tungsten is chosen where a dense, heat-resistant precious metal is needed in wire form. Heraeus lists PtW8 for spark plug electrodes, resistance wire and medical wire, and Goodfellow lists the same composition for furnace heater wire, sensor assemblies and probe tips. Platinum-copper appears in the sources as a laboratory catalyst for acid fuel-cell reactions. The bulk alloy's properties are not in the sources read here.

Where it's used

Spark plug electrodes

Heraeus lists PtW8 for spark plug electrodes, supplied as wire.

Furnace and heater wire

Goodfellow lists Pt92/W8 for specialised resistance wiring in high-temperature furnaces and for precision heater coils.

Sensors and probe tips

Goodfellow lists Pt92/W8 for advanced sensor assemblies, microfabricated probe tips and high-vacuum electrical feedthroughs.

Fuel-cell catalyst (laboratory)

A 2021 study reports a peak methanol oxidation current of 1236 A/g(Pt) for dealloyed PtCu/C, against 350 A/g(Pt) for a commercial Pt/C reference, in 0.1 M HClO4 with methanol.

Recipe

Pt-8W: platinum with 8 % tungsten by mass (Pt92/W8). Pt-Cu: carbon-supported PtCux nanoparticles, x = 1.3 by XRF before activation

Pt-8W is a binary alloy of platinum and tungsten, 92 % platinum and 8 % tungsten by mass. The Heraeus datasheet calls the same grade PtW8 and gives no composition; the 8 % figure comes from the Goodfellow and Calfine product names. Platinum-copper has no fixed bulk composition in these sources. The catalyst studied has a Cu to Pt ratio of 1.3 by XRF before activation, and its lattice parameter gives a Vegard composition of PtCu0.54.

What Pt-W, Pt-Cu is made of
IngredientShare of the weightWhat it does
Platinum Pt 92% The matrix metal, about 92 % by mass. The Heraeus datasheet gives a density of 21.26 g/cm3 for the alloy.
Tungsten W 8% The minor element, about 8 % by mass. The datasheet gives tensile strength of 800 to 1100 MPa for the alloy, but does not say what tungsten contributes.

Weight shares are as printed in the sources.

What it can do

Density

21.26 g/cm3

measured

The PtW8 wire has a density of 21.26 g/cm3 in the Heraeus datasheet. Goodfellow gives 21.3 g/cm3 for Pt92/W8.

Melting

1865 to 1885 °C

measured

Heraeus gives a melting range of 1865 to 1885 °C for PtW8. Goodfellow gives 1870 to 1910 °C for Pt92/W8.

Hardness

200 to 300 HV

measured

The Heraeus datasheet gives 200 to 300 HV for PtW8, with tensile strength of 800 to 1100 MPa.

Catalyst activity

1236 A/g(Pt)

measured

The dealloyed PtCu/C catalyst gave a peak methanol oxidation current of 1236 A/g(Pt), against 350 A/g(Pt) for the commercial reference, in one laboratory study.

How it compares

Platinum-tungsten is a heavy, high-melting wire metal with low electrical conductivity (2.58 to 2.77 % IACS in the Heraeus datasheet). The Heraeus datasheet gives its melting range as 1865 to 1885 °C. The rows below show the bulk alloy's density, melting range and modulus where a source gives them; no comparison with other materials was read in this run.

The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.

Benchmarks
MeasurementPt-W, Pt-CuAuAgPtPdRhRuOsAu alloysAuSnAg 92.5 Cu 7.5Ag alloysPd-AgPd-Cu, Pd-Ni, Pd-CrPt-RhPt-Ir
Thermal behavior and safety
Melting range, PtW8 (Heraeus Hera 158)Range printed in a manufacturer datasheet1865 to 1885 °C1065 °C961.9 °C1769 °C1555 °C1964 °C2334 °C3033 °C955 °C280 °C788 to 891 °C780 °Cno data1397 °C1840 to 1870 °C1790 to 1800 °C
Melting range, Pt92/W8 (Goodfellow)Range printed on a reseller product page1870 to 1910 °C1065 °C961.9 °C1769 °C1555 °C1964 °C2334 °C3033 °C955 °C280 °C788 to 891 °C780 °Cno data1397 °C1840 to 1870 °C1790 to 1800 °C
Physical and electrical
Density, PtW8 wire (Heraeus Hera 158)Value printed in a manufacturer datasheet21.26 g/cm³19.3 g/cm³10.5 g/cm³21.45 g/cm³12.02 g/cm³12.42 g/cm³12.36 g/cm³22.5 g/cm³15.8 g/cm³14.7 -10.4 g/cm³10 Mg/m310.9 g/cm³10.8 g/cm³19.97 g/cm³21.54 g/cm³
Density, Pt92/W8 wire (Goodfellow)Value printed on a reseller product page21.3 g/cm³19.3 g/cm³10.5 g/cm³21.45 g/cm³12.02 g/cm³12.42 g/cm³12.36 g/cm³22.5 g/cm³15.8 g/cm³14.7 -10.4 g/cm³10 Mg/m310.9 g/cm³10.8 g/cm³19.97 g/cm³21.54 g/cm³
Hardness HV, PtW8 (Heraeus Hera 158)Range printed in a manufacturer datasheet200 to 300 HVno datano data42 HV40 HVno data750 kgf/mm2300 to 350 kgf/mm2no datano datano datano data55 HV580 to 620 HVno data105 HV
Electrical conductivity range, PtW8 (Heraeus Hera 158)2.58 to 2.77 % IACS14.5×10^7 S/mno data15.78 to 16.07 % IACSno datano datano datano datano datano datano datano datano datano datano data6.83 to 7.02 % IACS
Electrical resistivity, Pt92/W8 (Goodfellow)Range printed on a reseller product page62 to 68 µOhm cm2.2×10^-8 ohm m1.63 µΩ·cm10.6 µΩ·cm10.8 uOhm.cm43.3 nΩ·m71 nΩ·m8.8 µΩ·cm15.5 µΩ·cmno data1.8 µOhmcm20.4 x10-9 ohm m15 uOhm.cmno datano datano data
Temperature behavior
Temperature coefficient of resistance, Pt92/W8 (Goodfellow)Value printed on a reseller product page2.5×10^-4 K-12no datano data0.0039 /°Cno datano datano datano datano datano datano datano datano datano datano datano data
Other measurements
Tensile strength, PtW8 (Heraeus Hera 158)Range printed in a manufacturer datasheet800 to 1100 MPano datano data150 MPano datano datano datano data616 MPa275 MPa207 MPa372 MPa310 MPano data300 to 680 MPa340 MPa
Yield strength, PtW8 (Heraeus Hera 158)Range printed in a manufacturer datasheet400 to 1000 MPano datano data70 MPano datano datano datano datano datano datano data272 MPa150 MPano data180 to 670 MPa220 MPa
Elongation, PtW8 (Heraeus Hera 158)Range printed in a manufacturer datasheet2 to 20 %no datano data40 %no datano datano datano data13 %no datano data19 %36 %3 %1.5 to 32 %32 %
Modulus of elasticity, Pt92/W8 (Goodfellow)Value printed on a reseller product page230 GPano datano data170 GPa121 GPa380 GPa447 GPa559 GPano data68 GPano data80 to 85 GPa114 GPano data208 GPa202.3 GPa
Electrochemically active surface area, PtCu/C activated 0.04 to 1.20 V41 m2/g(Pt)3no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Electrochemically active surface area, PtCu/C activated 0.04 to 1.00 V43 m2/g(Pt)4no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Peak methanol oxidation current, PtCu/C activated 0.04 to 1.00 V1236 A/g(Pt)5no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Peak methanol oxidation current, commercial Pt/C reference (JM20)350 A/g(Pt)6no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Lattice parameter a, PtCu/C from XRD3.815 Å7no datano datano data3.891 angstromno datano datano datano datano datano datano datano datano datano datano data
XRD crystallite size, PtCu/C (Scherrer)2.7 nm8no datano datano datano datano datano datano datano datano datano datano datano datano datano datano data

Why choose it, and why not

Good for

  • Heat-resistant wire where density is acceptable. Heraeus lists PtW8 for resistance wire and spark plug electrodes.
  • Sensor and probe wire. Goodfellow lists Pt92/W8 for sensor assemblies and microfabricated probe tips.
  • Laboratory fuel-cell catalyst research on dealloyed PtCu/C, in acid electrolyte.

Watch out for

  • Heavy for its size at 21.26 g/cm3.
  • Low conductivity, 2.58 to 2.77 % IACS in the datasheet.
  • The PtCu catalyst loses copper in acid during activation. The composition moves from PtCu1.3 to about PtCu0.25.
  • No bulk Pt-Cu density, melting point or hardness was read in this run.

Platinum-tungsten is a dense, oxidation-resistant wire metal with datasheet values for density, melting range and mechanical strength. Platinum-copper is only covered here as a catalyst, and the bulk alloy needs a handbook source before it is used.

Technical details

For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.

Other names and standards

The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.

Other names and standards
SystemCodes
Trade namePtW8, Hera 158

Notes

The method, full conditions and any caveat for the numbered rows above.

Notes for the numbered rows
#MeasurementMethodConditionsCaveat
1Electrical conductivity range, PtW8 (Heraeus Hera 158)Minimum and maximum printed in a manufacturer datasheet. The datasheet prints the minimum (2.77) above the maximum (2.58), so the range is entered low to high. Check the datasheet before using either end.form PtW8 wiretemperature not stated in the datasheet—
2Temperature coefficient of resistance, Pt92/W8 (Goodfellow)—form Pt92/W8 wiretemperature range not stated on the pageNon-canonical name; add to property-canon if kept.
3Electrochemically active surface area, PtCu/C activated 0.04 to 1.20 VValue printed in a 2021 open-access paper, Table 1form carbon-supported PtCu/C catalyst, nominal PtCu1.3 before activationelectrolyte 0.1 M HClO4activation 100 voltammetric cycles, 0.04 to 1.20 V vs RHE, 200 mV/sNon-canonical name.
4Electrochemically active surface area, PtCu/C activated 0.04 to 1.00 VValue printed in a 2021 open-access paper, Table 1form carbon-supported PtCu/C catalyst, nominal PtCu1.3 before activationelectrolyte 0.1 M HClO4activation 100 voltammetric cycles, 0.04 to 1.00 V vs RHE, 200 mV/sNon-canonical name.
5Peak methanol oxidation current, PtCu/C activated 0.04 to 1.00 VValue printed in a 2021 open-access paper, Table 2electrolyte 0.1 M HClO4 with 0.5 M CH3OH, argonscan 20 mV/s, 0.04 to 1.3 V vs RHENon-canonical name. Normalised to platinum mass by the authors.
6Peak methanol oxidation current, commercial Pt/C reference (JM20)Value printed in a 2021 open-access paper, Table 2electrolyte 0.1 M HClO4 with 0.5 M CH3OH, argonscan 20 mV/s, 0.04 to 1.3 V vs RHENon-canonical name. Reference catalyst for the comparison above.
7Lattice parameter a, PtCu/C from XRDValue calculated and printed in a 2021 open-access paperform PtCu/C catalyst, Pt-Cu solid solutionmethod XRD with Vegard's lawNon-canonical name. The same sentence gives the composition PtCu0.54 by Vegard's law.
8XRD crystallite size, PtCu/C (Scherrer)Value printed in a 2021 open-access paper; plus or minus 0.1 nm printedform PtCu/C catalystmethod Scherrer equation from XRDNon-canonical name. TEM gives a nanoparticle size of about 5 nm, which the authors say is larger than the XRD crystallite size.

Corrosion and compatibility

What happens when it meets other materials and environments.

Corrosion and compatibility
EnvironmentConcernWhat happens
Air at high temperature (PtW8 wire) low Heraeus lists PtW8 as oxidation resistant to 1000 °C.1
Acid electrolyte with electrochemical cycling (PtCu/C catalyst) moderate Copper leaves the PtCu/C surface during activation in acid, and the copper content falls.2
Corrosion details
#EnvironmentDetailsTest conditions
1 Air at high temperature (PtW8 wire) The datasheet gives this as a chemical-property comment with no test method, atmosphere, exposure time or oxidation rate. basis qualitative datasheet statement onlylimit 1000 °C as printed
2 Acid electrolyte with electrochemical cycling (PtCu/C catalyst) After 100 voltammetric cycles in 0.1 M HClO4, the Cu to Pt ratio fell from PtCu1.3 to PtCu0.25 after activation to 1.20 V, and to PtCu0.24 after activation to 1.00 V. The authors call this de-alloying. The text read here does not report Pt or Cu dissolved into the electrolyte. electrolyte 0.1 M HClO4cycling 100 cycles at 200 mV/s, 0.04 to 1.20 V or 0.04 to 1.00 V vs RHEcomposition basis after the activation stage, as printed in Table 1

Risks and side effects

Hazards to people, what happens when a cell overheats, and how the material is handled and stored.

For people

The platinum, tungsten and copper element records carry flammable, irritant or aquatic codes in some company reports. The alloys have no record of their own.

Platinum element
Of 504 company reports, 410 said platinum does not meet GHS criteria. H228 (flammable solid, 10.7 %) is shown, and H334 (respiratory sensitisation) comes from the notifications.
Tungsten element
Of 741 company reports, 196 said tungsten does not meet GHS criteria. H228 (73.4 %) and H252 (47.8 %, self-heating in large quantities) are shown, with H320 and H335.
Copper element
Of 3463 company reports, 1818 said copper does not meet GHS criteria. Notified codes include H400 (43.1 %) and H410 (18.8 %), which concern aquatic life, and H302 (21.7 %).

If it fails

The only failure route in a read source is copper loss from the catalyst in acid, found in a laboratory study.

Catalyst activation
In the 2021 study, 100 cycles in 0.1 M HClO4 took the Cu to Pt ratio from 1.3 to about 0.25. The two activation windows gave the same composition but different kinetic currents, so the surface state matters as well as the composition.

Handling and storage

Forming
Heraeus lists PtW8 as ductile and formable, but hardly formable, and as not age hardenable. It is machinable.
Heat
The datasheet lists oxidation resistance to 1000 °C. It gives no test conditions.

Test details
The original wording and numbers from the sources, for readers who want them.

Failure risks

Failure risks
FailureTrigger and consequence
Copper loss from the PtCu catalyst surface in acidmoderate severityElectrochemical activation cycling in 0.1 M HClO4Copper falls to a Cu to Pt ratio of about 0.25 after activation in both windows, while the activation window changes the kinetic current (417 and 878 A/g(Pt) in Table 1). The authors attribute the activity difference to surface structure, not composition.

Side effects on surrounding parts

Side effects on surrounding parts
AffectsEffect
Mass of electrodes, probes and wire assembliesPtW8 density is 21.26 g/cm3, so parts are heavy for their size.

Handling and storage

  • Heraeus lists PtW8 as ductile, formable and machinable, but hardly formable, and as not age hardenable.

Supply and geography

How common the raw materials are and where they come from.

Platinum (world mine production, used for the platinum content)

Top producers (2025)
South Africa 70.6%, Russia 11.8%, Zimbabwe 10.6%, Canada 2.9%, United States 1.1%
Recycling
USGS: about 140,000 kg of palladium and platinum were recovered globally from new and old scrap in 2025.

Tungsten

Top producers (2025)
China 78.8%, Vietnam 3.5%, Kazakhstan 2.8%, Russia 2.4%, Korea, North 2.4%
Recycling
USGS: the quantity of secondary tungsten produced and consumed in 2025 was withheld to avoid disclosing company data.
Substitutes
USGS: molybdenum can replace tungsten in some mill products, and depleted uranium or lead can replace tungsten alloys where high density or radiation shielding is needed.

Copper

Top producers (2025)
Chile 23%, Congo (Kinshasa) 13.9%, Peru 11.7%, China 7.8%, Russia 5.7%
Critical mineral lists
US: listed
Recycling
USGS: old scrap gave an estimated 160,000 tons of copper in the United States in 2025.
Substitutes
USGS: aluminum substitutes for copper in several electrical and cooling uses, and optical fiber substitutes for copper in telecommunications.