Titanium hydride TiH2
TiH2 (titanium dihydride), ZrH2 (zirconium dihydride) and HfH2 (hafnium dihydride). Albemarle lists the molecular formula TiH2 for grade N and ZrH2 for grade PS. The Bangor paper writes the hafnium phase as HfH2-x, and the INL review writes zirconium hydride phases as ZrH1.6 and ZrH1.85 · CAS 7704-98-5
This profile covers three metal dihydrides that share one powder form and one behaviour: titanium hydride (TiH2), zirconium hydride (ZrH2) and hafnium hydride (HfH2).
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Hydrogen density
0.152
Moderation
55
Density
3.91
Recipe, share of the weight
- Ti 15.0%Titanium
- Zr 28.5%Zirconium
- Hf 55.8%Hafnium
- H 0.6%Hydrogen
Best for
Hydrogen reservoirs and foaming agents for metal powder processing (Albemarle grade N and the KTU aluminium foam paper), and zirconium hydride as a moderator with a high moderating ratio (ORNL Table 1)
Weakest at
Hydrogen loss on heating: TiH2 releases hydrogen from about 763 K, ZrH2 evolves hydrogen above 300 °C (ATI), and all three powders are flammable with a dust-explosion risk
Risk at a glance
- People None found. Flammable powder with a dust-explosion risk
- If it fails High. Dust cloud or powder ignition
- Corrosion Moderate. TiH2 resists most reagents but oxidizing agents, acids and cold hydrofluoric acid attack it
Quick facts: TiH2
| Property | Value | Basis |
|---|---|---|
| Density | 3.78 to 11.4 g/cm³ | 6 sourced values across conditions |
| Melting point | at least 400 °C | 1 sourced value |
What is the density of Titanium hydride (TiH2)?
Titanium hydride (TiH2) has a density of 3.78 to 11.4 g/cm³. The range covers 6 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the melting point of Titanium hydride (TiH2)?
Titanium hydride (TiH2) has a melting point of at least 400 °C. The source and test conditions are listed in the properties table on this page.
What is Titanium hydride (TiH2) used for?
Uses recorded in the sources include Titanium hydride as a reservoir for pure hydrogen; Zirconium hydride moderator in SNAP and TRIGA reactors; Hafnium hydride neutron moderator and attenuator for compact reactors.
Why it exists
Titanium hydride and its zirconium and hafnium relatives store a large amount of hydrogen in a dense solid. Albemarle sells TiH2 as a reservoir for pure hydrogen, a hydrogen source for foaming metals and an alloying aid in powder metallurgy. ZrH2 has long been the moderator of choice for compact reactors, because it combines a high moderating ratio (55 in ORNL Table 1) with hydrogen density. HfH2 is studied as a moderator and attenuator for compact reactors. The trade is that all three release hydrogen when heated, so their use depends on keeping the hydrogen in place.
Where it's used
Hydrogen reservoir
Albemarle says TiH2 is used as a reservoir for pure hydrogen and yields hydrogen at elevated temperatures in a reversible reaction. The ORNL report describes metal hydrides as a low-risk option for dense hydrogen storage.
Reactor moderators
ORNL names the SNAP program and TRIGA reactors as users of zirconium hydride as a moderator. The Bangor abstract calls hafnium hydride a candidate moderator and attenuator for compact reactors.
Foaming and powder metallurgy
The KTU paper foams commercially pure aluminium with 1.5 wt% TiH2 to a porosity of about 80 %. Albemarle lists the ZrH2 and HfH2 grades as hydrogen sources for foaming metals and as alloying additions in powder metallurgy.
Recipe
TiH2 (titanium dihydride), ZrH2 (zirconium dihydride) and HfH2 (hafnium dihydride). Albemarle lists the molecular formula TiH2 for grade N and ZrH2 for grade PS. The Bangor paper writes the hafnium phase as HfH2-x, and the INL review writes zirconium hydride phases as ZrH1.6 and ZrH1.85
TiH2, ZrH2 and HfH2 each have one metal atom and two hydrogen atoms per formula unit. The metal is bonded to hydrogen in a hydride lattice that expands on hydriding (ORNL). The common preparation is direct reaction of the metal with hydrogen gas, guided by the phase diagram (ORNL); no process temperature for these grades was sourced.
| Ingredient | Atoms per unit | Share of the weight | What it does |
|---|---|---|---|
| Titanium Ti | 1 | 15.0% | Metal in TiH2. NIST gives 47.867 (1). |
| Zirconium Zr | 1 | 28.5% | Metal in ZrH2. NIST gives 91.224 (2). |
| Hafnium Hf | 1 | 55.8% | Metal in HfH2. NIST gives 178.49 (2). |
| Hydrogen H | 2 | 0.6% | Stored in the lattice and released on heating. NIST gives [1.00784, 1.00811] as the standard atomic weight, so 1.008 is used. |
Weight shares are calculated from standard atomic weights.
What it can do
Hydrogen density
0.152
measured
TiH2 holds 0.152 g of hydrogen per cm3 of hydride, and ZrH2 holds 0.122 g per cm3, both from ORNL Table 1.
Moderation
55
measured
In ORNL Table 1, ZrH2 has a moderating ratio of 55 against 6.3 for TiH2. The ratio measures slowing-down power against neutron absorption.
Density
3.91
measured
TiH2 has a density of 3.91 g/cm3 at 20 °C (Albemarle). ZrH2 is 5.6 g/cm3 at 25 °C and HfH2 is 11.4 g/cm3 at 20 °C (Albemarle grades).
How it compares
The three hydrides are light and dense in hydrogen content, but they differ in density by a factor of about three. TiH2 is the least dense, which suits powder metallurgy. ZrH2 has the highest moderating ratio of the three tabulated in ORNL and it is the moderator in SNAP-type reactors. HfH2 is the densest and releases hydrogen in steps near 350, 415 and 700 °C. The three are compared on density, hydrogen content and hydrogen density because those are the values that all sources give.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | TiH2 | W | WC | Hf | Mo | Mo-Re | Mo-30W | TZM | Nb | Nb alloys | Re | W-Re | WHA | W-Cu | W-Ag | WT20 | V | V alloys | Zr | Zr alloys | Be |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Capacity and energy | |||||||||||||||||||||
| Kissinger activation energy, first desorption step, HfH2-x | 150 kJ/mol25 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Kissinger activation energy, second desorption step, HfH2-x | 170 kJ/mol26 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Kissinger activation energy, third desorption step, HfH2-x | 90 kJ/mol27 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Thermal behavior and safety | |||||||||||||||||||||
| Melting point range, TiH2 (decomposes before melting) | > 400 °C6 | 3695 K | no data | 2233 °C | 2623 °C | > 2610 °C | 2829 °C | no data | 2477 °C | 2350 °C | 3186 °C | 3350 °C | no data | no data | no data | 3695 K | 1910 °C | 1900 °C | 1852 °C | 1850 °C | 1287 °C |
| Hydrogen evolution onset, ZrH2 | > 300 °C18 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Lifetime and stability | |||||||||||||||||||||
| Volume expansion on hydriding, TiH2 | 19 %9 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Volume expansion on hydriding, ZrH2 | 14.3 %13 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Physical and electrical | |||||||||||||||||||||
| Density, TiH2 powder, 20 °C | 3.91 g/cm³1 | 19250 kg/m3 | 14.8 g/cm³ | 13.3 g/cm³ | 10.22 g/cm³ | 14.6 g/cm³ | 10.9 g/cm³ | 10.2 g/cm³ | 8.582 g/cm³ | 8.85 g/cm³ | 21.02 g/cm³ | 19.4 g/cm³ | 16.85 to 17.25 g/cc | 15.15 g/cm³ | 11.75 to 16.1 g/cm³ | 19250 kg m-3 | 6.11 g/cm³ | 6.05 g/cm³ | 6.51 g/cm³ | 6.55 g/cc | 1.85 g/cm³ |
| Density, TiH2, 25 °C (supplier SDS) | 3.91 g/cm³2 | 19250 kg/m3 | 14.8 g/cm³ | 13.3 g/cm³ | 10.22 g/cm³ | 14.6 g/cm³ | 10.9 g/cm³ | 10.2 g/cm³ | 8.582 g/cm³ | 8.85 g/cm³ | 21.02 g/cm³ | 19.4 g/cm³ | 16.85 to 17.25 g/cc | 15.15 g/cm³ | 11.75 to 16.1 g/cm³ | 19250 kg m-3 | 6.11 g/cm³ | 6.05 g/cm³ | 6.51 g/cm³ | 6.55 g/cc | 1.85 g/cm³ |
| Hydride density, TiH2, ORNL Table 1 | 3.78 g/cm³3 | 19250 kg/m3 | 14.8 g/cm³ | 13.3 g/cm³ | 10.22 g/cm³ | 14.6 g/cm³ | 10.9 g/cm³ | 10.2 g/cm³ | 8.582 g/cm³ | 8.85 g/cm³ | 21.02 g/cm³ | 19.4 g/cm³ | 16.85 to 17.25 g/cc | 15.15 g/cm³ | 11.75 to 16.1 g/cm³ | 19250 kg m-3 | 6.11 g/cm³ | 6.05 g/cm³ | 6.51 g/cm³ | 6.55 g/cc | 1.85 g/cm³ |
| Hydrogen density, TiH2Printed in ORNL Table 1, TiH2 row | 0.152 g H/cm³ | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Density, ZrH2 powder, 25 °C | 5.6 g/cm³10 | 19250 kg/m3 | 14.8 g/cm³ | 13.3 g/cm³ | 10.22 g/cm³ | 14.6 g/cm³ | 10.9 g/cm³ | 10.2 g/cm³ | 8.582 g/cm³ | 8.85 g/cm³ | 21.02 g/cm³ | 19.4 g/cm³ | 16.85 to 17.25 g/cc | 15.15 g/cm³ | 11.75 to 16.1 g/cm³ | 19250 kg m-3 | 6.11 g/cm³ | 6.05 g/cm³ | 6.51 g/cm³ | 6.55 g/cc | 1.85 g/cm³ |
| Hydride density, ZrH2, ORNL Table 1 | 5.56 g/cm³11 | 19250 kg/m3 | 14.8 g/cm³ | 13.3 g/cm³ | 10.22 g/cm³ | 14.6 g/cm³ | 10.9 g/cm³ | 10.2 g/cm³ | 8.582 g/cm³ | 8.85 g/cm³ | 21.02 g/cm³ | 19.4 g/cm³ | 16.85 to 17.25 g/cc | 15.15 g/cm³ | 11.75 to 16.1 g/cm³ | 19250 kg m-3 | 6.11 g/cm³ | 6.05 g/cm³ | 6.51 g/cm³ | 6.55 g/cc | 1.85 g/cm³ |
| Hydrogen density, ZrH2Printed in ORNL Table 1, ZrH2 row | 0.122 g H/cm³ | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Density, HfH2 powder, 20 °C | 11.4 g/cm³19 | 19250 kg/m3 | 14.8 g/cm³ | 13.3 g/cm³ | 10.22 g/cm³ | 14.6 g/cm³ | 10.9 g/cm³ | 10.2 g/cm³ | 8.582 g/cm³ | 8.85 g/cm³ | 21.02 g/cm³ | 19.4 g/cm³ | 16.85 to 17.25 g/cc | 15.15 g/cm³ | 11.75 to 16.1 g/cm³ | 19250 kg m-3 | 6.11 g/cm³ | 6.05 g/cm³ | 6.51 g/cm³ | 6.55 g/cc | 1.85 g/cm³ |
| Temperature behavior | |||||||||||||||||||||
| Auto-ignition temperature, TiH2 powder | > 400 °C7 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Hydrogen release onset, untreated TiH2 | 763 K8 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Hydrogen desorption step near 350 °C, HfH2-x | 350 °C22 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Hydrogen desorption step near 415 °C, HfH2-x | 415 °C23 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Hydrogen desorption step near 700 °C, HfH2-x | 700 °C24 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Other measurements | |||||||||||||||||||||
| Molar mass, TiH2 | 49.88 g/mol4 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Hydrogen content, TiH2 grade N, minimum | 3.8 %5 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Moderating ratio, TiH2Printed in ORNL Table 1, TiH2 row | 6.3 - | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Moderating ratio, ZrH2 | 55 -12 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Slowing-down power, ZrH2Printed in ORNL Table 1, ZrH2 row | 1.45 - | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Hydrogen content, ZrH2 grade PS, minimum | 1.5 %14 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Hydrogen content, ZrH2 grade G, minimum | 1.9 %15 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Dissociation pressure, epsilon ZrH1.85 at 800 °C | 30 atm16 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Dissociation pressure, delta ZrH1.6 at 800 °C | 1 atm17 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Hydrogen content, HfH2 grade PS, minimum | 1 %20 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
| Molar mass, HfH2 grade PS | 180.5 g/mol21 | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data | no data |
Why choose it, and why not
Good for
- Hydrogen reservoirs and foaming agents, where a dense, stable powder that gives off hydrogen on heating is wanted (Albemarle, KTU).
- Compact-reactor moderators, where ZrH2 has a high moderating ratio (ORNL Table 1) and HfH2 is studied as a moderator and attenuator (Bangor).
Watch out for
- Hydrogen loss on heating: TiH2 near 763 K, ZrH2 above 300 °C, and HfH2 in steps near 350, 415 and 700 °C.
- Dust explosion and flammability. All three are flammable solids and the powder is dangerous in a dust cloud.
- The density of TiH2 differs by source: 3.91 g/cm3 from Albemarle and Sigma, and 3.78 g/cm3 in ORNL Table 1.
Metal hydride powders are a good hydrogen store and foaming agent, and ZrH2 is a proven reactor moderator. They give off hydrogen on heating and burn as dust, so each use needs the hydrogen kept in place and the powder kept from ignition. Melting, hardness, thermal conductivity and flight data are not sourced here.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Density, TiH2 powder, 20 °C | Density printed in the Albemarle grade N technical data sheet, method OPPTS 830.7300 | temperature 20 °Cform powder, grade N | — |
| 2 | Density, TiH2, 25 °C (supplier SDS) | Relative density printed in the Sigma-Aldrich SDS, physical and chemical properties section | temperature 25 °C (77 °F) | — |
| 3 | Hydride density, TiH2, ORNL Table 1 | Printed in the ORNL Table 1 column Hydride density (g/cm3). It differs from the 3.91 g/cm3 manufacturer values and is kept as printed | basis hydride density as tabulated by ORNL, which cites a reference for the table | — |
| 4 | Molar mass, TiH2 | Molecular weight printed in the Sigma-Aldrich SDS | basis molecular weight printed in the supplier SDS, formula H2Ti | — |
| 5 | Hydrogen content, TiH2 grade N, minimum | Specification minimum printed in the Albemarle grade N data sheet | grade Nbound minimum | — |
| 6 | Melting point range, TiH2 (decomposes before melting) | Printed as greater than 400 °C with the note decomposes before melting | basis decomposes before melting | — |
| 7 | Auto-ignition temperature, TiH2 powder | Printed as greater than 400 °C in the Albemarle grade N specification. The Sigma-Aldrich SDS gives no auto-ignition data | form powder, grade N, min. 99.9 % below 63 µm | — |
| 8 | Hydrogen release onset, untreated TiH2 | Secondhand figure quoted in the KTU paper introduction. Kept in kelvin as printed | basis approximately 763 K for untreated TiH2, as cited by the paper from Kennedy et al. | — |
| 9 | Volume expansion on hydriding, TiH2 | Printed in the ORNL introduction (e.g., 19% in the case of TiH2) | basis metal to hydride transformation, as printed for TiH2 | — |
| 10 | Density, ZrH2 powder, 25 °C | Density printed in the Albemarle grade PS technical data sheet, with the note information taken from reference works and the literature | temperature 25 °Cform powder, grade PS | — |
| 11 | Hydride density, ZrH2, ORNL Table 1 | Printed in ORNL Table 1, ZrH2 row, Hydride density column | basis hydride density as tabulated by ORNL | — |
| 12 | Moderating ratio, ZrH2 | Printed in ORNL Table 1, ZrH2 row. ORNL calls ZrHx the most promising moderator on this ratio | basis ratio of macroscopic slowing-down power to macroscopic neutron absorption cross section, as defined in the report | — |
| 13 | Volume expansion on hydriding, ZrH2 | Printed in the ORNL introduction (14.3% in the case of ZrH2) | basis metal to ZrH2 transformation, as printed | — |
| 14 | Hydrogen content, ZrH2 grade PS, minimum | Specification minimum printed in the Albemarle grade PS data sheet | grade PSbound minimum | — |
| 15 | Hydrogen content, ZrH2 grade G, minimum | Specification minimum printed in the Albemarle grade G data sheet | grade Gbound minimum | — |
| 16 | Dissociation pressure, epsilon ZrH1.85 at 800 °C | Phase stability entry printed in the INL and Los Alamos overview. The slide gives no further detail | phase epsilon, ZrH1.85temperature 800 °C | — |
| 17 | Dissociation pressure, delta ZrH1.6 at 800 °C | Phase stability entry printed in the INL and Los Alamos overview | phase delta, ZrH1.6temperature 800 °C | — |
| 18 | Hydrogen evolution onset, ZrH2 | Printed in the ATI safety data sheet, melting point and freezing point row | basis printed as evolves hydrogen above 300 °C | — |
| 19 | Density, HfH2 powder, 20 °C | Commercial powder specification printed on the Albemarle product page. It is not a measured value for pure stoichiometric HfH2 | temperature 20 °Cform powder, grade PS (technical grade) | — |
| 20 | Hydrogen content, HfH2 grade PS, minimum | Typical specification printed on the Albemarle product page | grade PSbound minimum | — |
| 21 | Molar mass, HfH2 grade PS | Printed as 180.50 g/mol in the Albemarle physical and chemical properties table | basis molecular weight printed on the Albemarle product page | — |
| 22 | Hydrogen desorption step near 350 °C, HfH2-x | Approximate step temperature printed in the Bangor abstract | phase epsilon, HfH2-xmethod isochronal heating by thermogravimetry from 25 to 1000 °C | — |
| 23 | Hydrogen desorption step near 415 °C, HfH2-x | Approximate step temperature printed in the Bangor abstract | phase delta, HfH1.6-xmethod isochronal heating by thermogravimetry from 25 to 1000 °C | — |
| 24 | Hydrogen desorption step near 700 °C, HfH2-x | Approximate step temperature printed in the Bangor abstract | phase alpha, Hfmethod isochronal heating by thermogravimetry from 25 to 1000 °C | — |
| 25 | Kissinger activation energy, first desorption step, HfH2-x | Approximate Kissinger value printed in the Bangor abstract | phase epsilon, HfH2-x | — |
| 26 | Kissinger activation energy, second desorption step, HfH2-x | Approximate Kissinger value printed in the Bangor abstract | phase delta, HfH1.6-x | — |
| 27 | Kissinger activation energy, third desorption step, HfH2-x | Approximate Kissinger value printed in the Bangor abstract | phase alpha, Hf | — |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Oxidizing agents, acids and cold hydrofluoric acid | moderate | TiH2 resists most reagents but oxidizing agents, acids and cold hydrofluoric acid attack it1 |
| Elevated temperature at low pressure | moderate | TiH2 gives off hydrogen on heating, so hydrogen loss must be planned for2 |
| Air, fine powder at room temperature | moderate | Fine ZrH2 powder burns slowly in air and must be kept from flames and sparks3 |
| Heating above 300 °C, and reversible hydrogen loss in vacuum | moderate | ZrH2 evolves hydrogen above 300 °C and its reaction runs back and forth in vacuum4 |
| Air, fine powder at room temperature | moderate | Fine HfH2 powder burns slowly in air and must not be fought with water5 |
| Heating from 25 to 1000 °C | moderate | HfH2 gives off hydrogen in three steps near 350, 415 and 700 °C6 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Oxidizing agents, acids and cold hydrofluoric acid | Albemarle says that like titanium metal, TiH2 resists most chemical reagents, but is attacked at elevated temperature by oxidizing agents and acids, and is attacked by cold hydrofluoric acid solutions. The rating moderate is the assistant's judgement from this statement. The sheet gives no test numbers. | basis statement in the handling section of the grade N data sheet |
| 2 | Elevated temperature at low pressure | Albemarle says that at elevated temperatures and low pressures the generation of hydrogen must be considered. The KTU paper gives 763 K as the release temperature for untreated TiH2 and reports that pre-treatment at 753 K for 30 min was best for aluminium foam. The rating moderate is the assistant's judgement; neither source rates it. | basis heating in the foaming process, and at low pressure per the data sheet |
| 3 | Air, fine powder at room temperature | Albemarle grade PS calls the powder a highly flammable solid with a dust explosion hazard that burns slowly in air. The sheet gives the handling rules: keep away from flames, sparks and heat sources, and use ground-connected apparatus to avoid ignition by electrostatic discharge. The rating moderate is the assistant's judgement. | basis handling statement in the grade PS data sheet, no test data |
| 4 | Heating above 300 °C, and reversible hydrogen loss in vacuum | The ATI sheet says ZrH2 evolves hydrogen above 300 °C. Albemarle grade PS says it yields hydrogen by a reversible reaction in vacuum. The INL overview says the hydrogen pressure in the cladding gives a higher burst risk for ZrH than for YH, and that no thermal testing data exist for ZrH in cladding. The rating moderate is the assistant's judgement. | basis heating and vacuum statements from two suppliers, and the INL overview of reactor moderators |
| 5 | Air, fine powder at room temperature | Albemarle grade PS for hafnium hydride calls it a highly flammable solid with a dust explosion hazard that burns slowly in air. Its fire guidance is to cover only with sand, limestone or a dry class D powder, and the sheet says do not use water. The rating moderate is the assistant's judgement. | basis handling instructions on the product page, no test data |
| 6 | Heating from 25 to 1000 °C | The Bangor study heats epsilon HfH2-x powder and finds three hydrogen release regions, one for each phase (epsilon HfH2-x, delta HfH1.6-x and alpha Hf). The study says hydrogen release degrades the moderating function, so the phase change matters for a moderator in service. The rating moderate is the assistant's judgement. | basis isochronal heating by thermogravimetry and X-ray diffraction; atmosphere not stated in the abstract |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
The three powders are sold as highly flammable solids with a dust-explosion hazard. The supplier sheets give the handling rules and the fire guidance.
- Ignition
- The Sigma-Aldrich SDS classifies TiH2 as a flammable solid with H228. Keep it away from flames, sparks and heat sources.
- Dust
- Albemarle warns of a dust explosion hazard for TiH2, ZrH2 and HfH2. Avoid dust and provide exhaust ventilation where dust is formed.
- Fire
- Cover a fire only with dry sand, limestone or a class D powder. Do not use water, carbon dioxide or halocarbon.
If a powder or part heats up
These results come from the sources listed, not from incidents.
- TiH2
- The KTU paper gives 763 K as the release temperature for untreated TiH2, and says that pre-treatment at 753 K for 30 min is the most suitable for aluminium foam.
- ZrH2
- ATI says ZrH2 evolves hydrogen above 300 °C. The INL overview gives a 30 atm dissociation pressure for the epsilon phase at 800 °C.
- HfH2
- The Bangor study finds hydrogen release near 350, 415 and 700 °C in three steps.
Handling and storage
- Storage
- Store dry and closed. ZrH2 grade PS is packed dry under argon in tins of at most 5 kg.
- Electrostatic discharge
- Use ground-connected metallic apparatus to avoid sudden ignition by electrostatic discharge (Albemarle).
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Dust cloud or powder ignitionhigh severity | Powder dispersed in air near a flame, spark or electrostatic dischargeAlbemarle warns of a dust explosion hazard and of sudden ignition by electrostatic discharge for the ZrH2 powder, and gives the same warning for TiH2 and HfH2 |
| Hydrogen release on heating, TiH2moderate severity | Heating above about 763 K in a melt or at low pressureThe hydrogen released forms bubbles that become pores in aluminium foam. Early release before the aluminium melts causes crack-like pores and loss of foaming control |
| Cladding burst, ZrH moderatorhigh severity | High-temperature operation of a ZrH moderator in claddingThe INL overview says ZrH has a higher plenum pressure and a higher burst risk than YH, and that no thermal testing data for ZrH in cladding are known |
| Loss of moderating function, HfH2moderate severity | Heating to about 350 °C and aboveThe Bangor abstract says hydrogen release leads to degradation of the moderating function of hafnium hydride |
Side effects on surrounding parts
| Affects | Effect |
|---|---|
| Equipment and people near a fire of hydride powder | At high temperature the hydrides release hydrogen, which is flammable. Albemarle and ATI both say that water on a fire can cause an explosion |
Handling and storage
- Keep away from flames, sparks and heat sources. Use ground-connected metallic apparatus to avoid sudden ignition by electrostatic discharge. Wear gloves, a face shield or goggles (ZrH2 grade PS, HfH2 product page)
- Use explosion-proof electrical, ventilating and lighting equipment (P241), and provide exhaust ventilation where dust is formed
- Packed dry under argon in tins of at most 5 kg (ZrH2 grade PS)
Mitigations
- Cover fires only with dry sand, limestone or a class D dry powder. Do not use water, carbon dioxide or halocarbon (TiH2 grade N, HfH2 product page)
Supply and geography
How common the raw materials are and where they come from.
Titanium (feedstock for TiH2)
- Top producers (2025)
- China 70.3%, Japan 14.3%, Russia 6.8%, Kazakhstan 4.3%, Saudi Arabia 3.2%
- Critical mineral lists
- EU: listed
- Recycling
- USGS 2026: consumption data for titanium scrap metal for the titanium metal industry were withheld, because survey responses were limited.
Zirconium (feedstock for ZrH2)
- Top producers (2025)
- Australia 33.3%, South Africa 22.5%, Mozambique 13.3%, China 8.3%, Senegal 5.8%
- Critical mineral lists
- EU: not listed
- Recycling
- USGS 2026: companies in Oregon and Utah recycled zirconium from new scrap generated during metal production. Refractories are often recycled but could not be quantified.
Hafnium (feedstock for HfH2)
- Critical mineral lists
- EU: listed
- Recycling
- USGS 2026: hafnium metal recycling was minimal.
- Substitutes
- USGS 2026: boron or cadmium-silver-indium alloys can substitute for hafnium metal in nuclear control rods, and zirconium can be used interchangeably with hafnium in certain superalloys.
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: titanium-hydride
spore_version: 0.2
family: refractory-metals
name: Titanium hydride
abbreviation: TiH2
role: hydrogen reservoir, foaming agent and neutron moderator (titanium, zirconium and hafnium hydrides)
category: metals
type: refractory-metals
summary: |
This profile covers three metal dihydrides that share one powder form and one behaviour: titanium hydride (TiH2), zirconium hydride (ZrH2) and hafnium hydride (HfH2). Albemarle grade N gives TiH2 a density of 3.91 g/cm3 at 20 °C, and its data sheet describes it as a reservoir for pure hydrogen and as a hydrogen source for foaming metals. Hydrogen comes out of the powder on heating: a KTU paper gives 763 K as the release temperature for untreated TiH2. ZrH2 was used as a moderator in the SNAP reactor program, and an INL and Los Alamos review gives a dissociation pressure of 30 atm at 800 °C for the epsilon phase of ZrH1.85. HfH2 powder releases hydrogen in three steps near 350, 415 and 700 °C (Bangor University).
best_for: Hydrogen reservoirs and foaming agents for metal powder processing (Albemarle grade N and the KTU aluminium foam paper), and zirconium hydride as a moderator with a high moderating ratio (ORNL Table 1)
weakest_at: 'Hydrogen loss on heating: TiH2 releases hydrogen from about 763 K, ZrH2 evolves hydrogen above 300 °C (ATI), and all three powders are flammable with a dust-explosion risk'
identity:
formula: TiH2 (titanium dihydride), ZrH2 (zirconium dihydride) and HfH2 (hafnium dihydride). Albemarle lists the molecular formula TiH2 for grade N and ZrH2 for grade PS. The Bangor paper writes the hafnium phase as HfH2-x, and the INL review writes zirconium hydride phases as ZrH1.6 and ZrH1.85
cas: 7704-98-5
source: albemarle-tih2-n
where: Title block, CAS-No. row (TiH2, grade N). CAS 7704-99-6 for ZrH2 (grade PS, Albemarle) and 12770-26-2 for HfH2 (Albemarle product page, metadata)
tags:
environments: []
stresses:
- extreme-heat
applications:
- propulsion-and-tanks
- radiation-shielding
- structures
properties:
- benchmark: density
label: Density, TiH2 powder, 20 °C
value: 3.91
unit: g/cm3
scope: material
conditions:
temperature: 20 °C
form: powder, grade N
method: Density printed in the Albemarle grade N technical data sheet, method OPPTS 830.7300
status: ground
source: albemarle-tih2-n
where: Physical and chemical properties table, Density row
- benchmark: density
label: Density, TiH2, 25 °C (supplier SDS)
value: 3.91
unit: g/cm3
scope: material
conditions:
temperature: 25 °C (77 °F)
method: Relative density printed in the Sigma-Aldrich SDS, physical and chemical properties section
status: ground
source: sigma-tih2
where: Physical and chemical properties, item m, Relative density
- benchmark: density
label: Hydride density, TiH2, ORNL Table 1
value: 3.78
unit: g/cm3
scope: material
conditions:
basis: hydride density as tabulated by ORNL, which cites a reference for the table
method: Printed in the ORNL Table 1 column Hydride density (g/cm3). It differs from the 3.91 g/cm3 manufacturer values and is kept as printed
status: ground
source: ornl-zrh-2020
where: Table 1, TiH2 row, Hydride density column
- benchmark: molar_mass
label: Molar mass, TiH2
value: 49.88
unit: g/mol
scope: material
conditions:
basis: molecular weight printed in the supplier SDS, formula H2Ti
method: Molecular weight printed in the Sigma-Aldrich SDS
status: ground
source: sigma-tih2
where: Composition or ingredients section, Molecular Weight row
- benchmark: hydrogen_content
label: Hydrogen content, TiH2 grade N, minimum
value: 3.8
unit: '%'
scope: material
conditions:
grade: 'N'
bound: minimum
method: Specification minimum printed in the Albemarle grade N data sheet
status: ground
source: albemarle-tih2-n
where: Specification table, Hydrogen row
- benchmark: melting_point
label: Melting point range, TiH2 (decomposes before melting)
value: 400
bound: lower
unit: °C
scope: material
conditions:
basis: decomposes before melting
method: Printed as greater than 400 °C with the note decomposes before melting
status: ground
source: albemarle-tih2-n
where: Physical and chemical properties table, Melting point/range row
- benchmark: auto_ignition_temperature
label: Auto-ignition temperature, TiH2 powder
value: 400
bound: lower
unit: °C
scope: material
conditions:
form: powder, grade N, min. 99.9 % below 63 µm
method: Printed as greater than 400 °C in the Albemarle grade N specification. The Sigma-Aldrich SDS gives no auto-ignition data
status: ground
source: albemarle-tih2-n
where: Specification table, Auto Ignition Temperature row
- benchmark: hydrogen_release_temperature
label: Hydrogen release onset, untreated TiH2
value: 763
unit: K
scope: material
conditions:
basis: approximately 763 K for untreated TiH2, as cited by the paper from Kennedy et al.
method: Secondhand figure quoted in the KTU paper introduction. Kept in kelvin as printed
status: ground
source: ktu-tih2-foam
where: Introduction, first paragraph
- benchmark: volume_change
label: Volume expansion on hydriding, TiH2
value: 19
unit: '%'
scope: material
conditions:
basis: metal to hydride transformation, as printed for TiH2
method: Printed in the ORNL introduction (e.g., 19% in the case of TiH2)
status: ground
source: ornl-zrh-2020
where: Section 1 Introduction, paragraph on volume expansion during hydriding
- benchmark: hydrogen_density
label: Hydrogen density, TiH2
value: 0.152
unit: g H/cm3
scope: material
conditions:
basis: mass of hydrogen per volume of hydride, as tabulated
method: Printed in ORNL Table 1, TiH2 row
status: ground
source: ornl-zrh-2020
where: Table 1, TiH2 row, g H/cm3 column
- benchmark: moderating_ratio
label: Moderating ratio, TiH2
value: 6.3
unit: '-'
scope: material
conditions:
basis: ratio of macroscopic slowing-down power to macroscopic neutron absorption cross section, as defined in the report
method: Printed in ORNL Table 1, TiH2 row
status: ground
source: ornl-zrh-2020
where: Table 1, TiH2 row, Moderating ratio column
- benchmark: density
label: Density, ZrH2 powder, 25 °C
value: 5.6
unit: g/cm3
scope: material
conditions:
temperature: 25 °C
form: powder, grade PS
method: Density printed in the Albemarle grade PS technical data sheet, with the note information taken from reference works and the literature
status: ground
source: albemarle-zrh-ps
where: Physical and chemical properties table, Density row
- benchmark: density
label: Hydride density, ZrH2, ORNL Table 1
value: 5.56
unit: g/cm3
scope: material
conditions:
basis: hydride density as tabulated by ORNL
method: Printed in ORNL Table 1, ZrH2 row, Hydride density column
status: ground
source: ornl-zrh-2020
where: Table 1, ZrH2 row, Hydride density column
- benchmark: hydrogen_density
label: Hydrogen density, ZrH2
value: 0.122
unit: g H/cm3
scope: material
conditions:
basis: mass of hydrogen per volume of hydride, as tabulated
method: Printed in ORNL Table 1, ZrH2 row
status: ground
source: ornl-zrh-2020
where: Table 1, ZrH2 row, g H/cm3 column
- benchmark: moderating_ratio
label: Moderating ratio, ZrH2
value: 55
unit: '-'
scope: material
conditions:
basis: ratio of macroscopic slowing-down power to macroscopic neutron absorption cross section, as defined in the report
method: Printed in ORNL Table 1, ZrH2 row. ORNL calls ZrHx the most promising moderator on this ratio
status: ground
source: ornl-zrh-2020
where: Table 1, ZrH2 row, Moderating ratio column
- benchmark: slowing_down_power
label: Slowing-down power, ZrH2
value: 1.45
unit: '-'
scope: material
conditions:
basis: as tabulated by ORNL, dimensionless
method: Printed in ORNL Table 1, ZrH2 row
status: ground
source: ornl-zrh-2020
where: Table 1, ZrH2 row, Slowing down power column
- benchmark: volume_change
label: Volume expansion on hydriding, ZrH2
value: 14.3
unit: '%'
scope: material
conditions:
basis: metal to ZrH2 transformation, as printed
method: Printed in the ORNL introduction (14.3% in the case of ZrH2)
status: ground
source: ornl-zrh-2020
where: Section 1 Introduction, paragraph on volume expansion during hydriding
- benchmark: hydrogen_content
label: Hydrogen content, ZrH2 grade PS, minimum
value: 1.5
unit: '%'
scope: material
conditions:
grade: PS
bound: minimum
method: Specification minimum printed in the Albemarle grade PS data sheet
status: ground
source: albemarle-zrh-ps
where: Specification table, H row
- benchmark: hydrogen_content
label: Hydrogen content, ZrH2 grade G, minimum
value: 1.9
unit: '%'
scope: material
conditions:
grade: G
bound: minimum
method: Specification minimum printed in the Albemarle grade G data sheet
status: ground
source: albemarle-zrh-g
where: Specification table, H row
- benchmark: dissociation_pressure
label: Dissociation pressure, epsilon ZrH1.85 at 800 °C
value: 30
unit: atm
scope: material
conditions:
phase: epsilon, ZrH1.85
temperature: 800 °C
method: Phase stability entry printed in the INL and Los Alamos overview. The slide gives no further detail
status: ground
source: inl-gain-2026
where: Phase stability slide, epsilon ZrH1.85 entry
- benchmark: dissociation_pressure
label: Dissociation pressure, delta ZrH1.6 at 800 °C
value: 1
unit: atm
scope: material
conditions:
phase: delta, ZrH1.6
temperature: 800 °C
method: Phase stability entry printed in the INL and Los Alamos overview
status: ground
source: inl-gain-2026
where: Phase stability slide, delta ZrH1.6 entry
- benchmark: hydrogen_evolution_onset
label: Hydrogen evolution onset, ZrH2
value: 300
bound: lower
unit: °C
scope: material
conditions:
basis: printed as evolves hydrogen above 300 °C
method: Printed in the ATI safety data sheet, melting point and freezing point row
status: ground
source: ati-zrh-sds
where: Physical and chemical properties table, Melting point/freezing point row
- benchmark: density
label: Density, HfH2 powder, 20 °C
value: 11.4
unit: g/cm3
scope: material
conditions:
temperature: 20 °C
form: powder, grade PS (technical grade)
method: Commercial powder specification printed on the Albemarle product page. It is not a measured value for pure stoichiometric HfH2
status: ground
source: albemarle-hfh-ps
where: Physical and chemical properties table, Density row
- benchmark: hydrogen_content
label: Hydrogen content, HfH2 grade PS, minimum
value: 1
unit: '%'
scope: material
conditions:
grade: PS
bound: minimum
method: Typical specification printed on the Albemarle product page
status: ground
source: albemarle-hfh-ps
where: Specifications list, H min row
- benchmark: molar_mass
label: Molar mass, HfH2 grade PS
value: 180.5
unit: g/mol
scope: material
conditions:
basis: molecular weight printed on the Albemarle product page
method: Printed as 180.50 g/mol in the Albemarle physical and chemical properties table
status: ground
source: albemarle-hfh-ps
where: Physical and chemical properties table, Molecular Weight row
- benchmark: hydrogen_desorption_temperature
label: Hydrogen desorption step near 350 °C, HfH2-x
value: 350
unit: °C
scope: material
conditions:
phase: epsilon, HfH2-x
method: isochronal heating by thermogravimetry from 25 to 1000 °C
method: Approximate step temperature printed in the Bangor abstract
status: ground
source: bangor-hfh
where: Abstract, first desorption region
- benchmark: hydrogen_desorption_temperature
label: Hydrogen desorption step near 415 °C, HfH2-x
value: 415
unit: °C
scope: material
conditions:
phase: delta, HfH1.6-x
method: isochronal heating by thermogravimetry from 25 to 1000 °C
method: Approximate step temperature printed in the Bangor abstract
status: ground
source: bangor-hfh
where: Abstract, second desorption region
- benchmark: hydrogen_desorption_temperature
label: Hydrogen desorption step near 700 °C, HfH2-x
value: 700
unit: °C
scope: material
conditions:
phase: alpha, Hf
method: isochronal heating by thermogravimetry from 25 to 1000 °C
method: Approximate step temperature printed in the Bangor abstract
status: ground
source: bangor-hfh
where: Abstract, third desorption region
- benchmark: activation_energy
label: Kissinger activation energy, first desorption step, HfH2-x
value: 150
unit: kJ/mol
scope: material
conditions:
phase: epsilon, HfH2-x
method: Approximate Kissinger value printed in the Bangor abstract
status: ground
source: bangor-hfh
where: Abstract, Kissinger analysis sentence
- benchmark: activation_energy
label: Kissinger activation energy, second desorption step, HfH2-x
value: 170
unit: kJ/mol
scope: material
conditions:
phase: delta, HfH1.6-x
method: Approximate Kissinger value printed in the Bangor abstract
status: ground
source: bangor-hfh
where: Abstract, Kissinger analysis sentence
- benchmark: activation_energy
label: Kissinger activation energy, third desorption step, HfH2-x
value: 90
unit: kJ/mol
scope: material
conditions:
phase: alpha, Hf
method: Approximate Kissinger value printed in the Bangor abstract
status: ground
source: bangor-hfh
where: Abstract, Kissinger analysis sentence
corrosion:
- environment: Oxidizing agents, acids and cold hydrofluoric acid
headline: TiH2 resists most reagents but oxidizing agents, acids and cold hydrofluoric acid attack it
effect: Albemarle says that like titanium metal, TiH2 resists most chemical reagents, but is attacked at elevated temperature by oxidizing agents and acids, and is attacked by cold hydrofluoric acid solutions. The rating moderate is the assistant's judgement from this statement. The sheet gives no test numbers.
rating: moderate
conditions:
basis: statement in the handling section of the grade N data sheet
source: albemarle-tih2-n
where: Handling and storage section
- environment: Elevated temperature at low pressure
headline: TiH2 gives off hydrogen on heating, so hydrogen loss must be planned for
effect: Albemarle says that at elevated temperatures and low pressures the generation of hydrogen must be considered. The KTU paper gives 763 K as the release temperature for untreated TiH2 and reports that pre-treatment at 753 K for 30 min was best for aluminium foam. The rating moderate is the assistant's judgement; neither source rates it.
rating: moderate
conditions:
basis: heating in the foaming process, and at low pressure per the data sheet
source: ktu-tih2-foam
where: Introduction and Section 3.1 Structural features
- environment: Air, fine powder at room temperature
headline: Fine ZrH2 powder burns slowly in air and must be kept from flames and sparks
effect: 'Albemarle grade PS calls the powder a highly flammable solid with a dust explosion hazard that burns slowly in air. The sheet gives the handling rules: keep away from flames, sparks and heat sources, and use ground-connected apparatus to avoid ignition by electrostatic discharge. The rating moderate is the assistant''s judgement.'
rating: moderate
conditions:
basis: handling statement in the grade PS data sheet, no test data
source: albemarle-zrh-ps
where: Handling row
- environment: Heating above 300 °C, and reversible hydrogen loss in vacuum
headline: ZrH2 evolves hydrogen above 300 °C and its reaction runs back and forth in vacuum
effect: The ATI sheet says ZrH2 evolves hydrogen above 300 °C. Albemarle grade PS says it yields hydrogen by a reversible reaction in vacuum. The INL overview says the hydrogen pressure in the cladding gives a higher burst risk for ZrH than for YH, and that no thermal testing data exist for ZrH in cladding. The rating moderate is the assistant's judgement.
rating: moderate
conditions:
basis: heating and vacuum statements from two suppliers, and the INL overview of reactor moderators
source: ati-zrh-sds
where: Physical and chemical properties table, Melting point/freezing point row
- environment: Air, fine powder at room temperature
headline: Fine HfH2 powder burns slowly in air and must not be fought with water
effect: Albemarle grade PS for hafnium hydride calls it a highly flammable solid with a dust explosion hazard that burns slowly in air. Its fire guidance is to cover only with sand, limestone or a dry class D powder, and the sheet says do not use water. The rating moderate is the assistant's judgement.
rating: moderate
conditions:
basis: handling instructions on the product page, no test data
source: albemarle-hfh-ps
where: Handling Instructions
- environment: Heating from 25 to 1000 °C
headline: HfH2 gives off hydrogen in three steps near 350, 415 and 700 °C
effect: The Bangor study heats epsilon HfH2-x powder and finds three hydrogen release regions, one for each phase (epsilon HfH2-x, delta HfH1.6-x and alpha Hf). The study says hydrogen release degrades the moderating function, so the phase change matters for a moderator in service. The rating moderate is the assistant's judgement.
rating: moderate
conditions:
basis: isochronal heating by thermogravimetry and X-ray diffraction; atmosphere not stated in the abstract
source: bangor-hfh
where: Abstract, desorption regions and degradation sentence
risks:
hazards:
- text: 'Sigma-Aldrich SDS: flammable solid, Category 1, hazard statement H228 (flammable solid), with the signal word Danger, and precautionary statement P241 (use explosion-proof electrical, ventilating and lighting equipment)'
ghs:
- H228
source: sigma-tih2
where: Section 2 Hazards identification; Section 2 Precautionary statements
- text: 'Albemarle grade N: highly flammable solid, dust explosion hazard. In case of fire, cover with dry sand or dry chemical, never with water, carbon dioxide or halocarbon'
ghs: []
source: albemarle-tih2-n
where: Handling and storage section
- text: 'ATI safety data sheet for zirconium hydride: flammable solids, Category 1, signal word Danger'
ghs: []
source: ati-zrh-sds
where: Section 2 Hazards identification, Label elements
- text: 'Albemarle hafnium hydride: highly flammable solid, dust explosion hazard. Do not use water on a fire'
ghs: []
source: albemarle-hfh-ps
where: Handling Instructions
failure_risks:
- mode: Dust cloud or powder ignition
trigger: Powder dispersed in air near a flame, spark or electrostatic discharge
consequence: Albemarle warns of a dust explosion hazard and of sudden ignition by electrostatic discharge for the ZrH2 powder, and gives the same warning for TiH2 and HfH2
severity: high
source: albemarle-zrh-ps
where: Handling row
- mode: Hydrogen release on heating, TiH2
trigger: Heating above about 763 K in a melt or at low pressure
consequence: The hydrogen released forms bubbles that become pores in aluminium foam. Early release before the aluminium melts causes crack-like pores and loss of foaming control
severity: moderate
source: ktu-tih2-foam
where: Introduction and Section 3 Results and discussion
- mode: Cladding burst, ZrH moderator
trigger: High-temperature operation of a ZrH moderator in cladding
consequence: The INL overview says ZrH has a higher plenum pressure and a higher burst risk than YH, and that no thermal testing data for ZrH in cladding are known
severity: high
source: inl-gain-2026
where: Main operational differences between YH and ZrH slide
- mode: Loss of moderating function, HfH2
trigger: Heating to about 350 °C and above
consequence: The Bangor abstract says hydrogen release leads to degradation of the moderating function of hafnium hydride
severity: moderate
source: bangor-hfh
where: Abstract, first paragraph
side_effects:
- text: At high temperature the hydrides release hydrogen, which is flammable. Albemarle and ATI both say that water on a fire can cause an explosion
affects: Equipment and people near a fire of hydride powder
source: ati-zrh-sds
where: Section 5 Extinguishing media
handling:
- text: Keep away from flames, sparks and heat sources. Use ground-connected metallic apparatus to avoid sudden ignition by electrostatic discharge. Wear gloves, a face shield or goggles (ZrH2 grade PS, HfH2 product page)
source: albemarle-zrh-ps
where: Handling row
- text: Use explosion-proof electrical, ventilating and lighting equipment (P241), and provide exhaust ventilation where dust is formed
source: sigma-tih2
where: Section 7 Handling and storage
- text: Packed dry under argon in tins of at most 5 kg (ZrH2 grade PS)
source: albemarle-zrh-ps
where: Packaging row
mitigations:
- text: Cover fires only with dry sand, limestone or a class D dry powder. Do not use water, carbon dioxide or halocarbon (TiH2 grade N, HfH2 product page)
source: albemarle-tih2-n
where: Handling and storage section
uses:
- application: propulsion-and-tanks
device: Titanium hydride as a reservoir for pure hydrogen
example: Albemarle lists TiH2 as a reservoir for pure hydrogen and says it yields hydrogen at elevated temperatures in a reversible reaction. The ORNL report says metal hydrides have been seen as an efficient, low-risk option for dense hydrogen storage since the late 1970s.
source: albemarle-tih2-n
where: Application section; Handling row
- application: radiation-shielding
device: Zirconium hydride moderator in SNAP and TRIGA reactors
example: The ORNL report names the SNAP program and TRIGA research reactors as users of ZrHx as a high-performance moderator. It ranks zirconium hydride as the most promising moderator of the hydrides it tabulates, on the moderating ratio.
source: ornl-zrh-2020
where: Section 1 Introduction, paragraph on moderator examples
- application: radiation-shielding
device: Hafnium hydride neutron moderator and attenuator for compact reactors
example: The Bangor University abstract calls hafnium hydride a candidate neutron moderator and attenuator for compact nuclear reactors, where hydrogen release would reduce its moderating performance.
source: bangor-hfh
where: Abstract, first sentence
- application: structures
device: Titanium hydride as a foaming agent for closed-cell aluminium foam
example: The KTU paper adds 1.5 wt% TiH2 to melted commercially pure aluminium and stirs it to make closed-cell foam with a porosity of about 80 %. The best pre-treatment was 753 K for 30 min.
source: ktu-tih2-foam
where: Section 2 Experimental, and Section 3.1 Structural features
- application: structures
device: Hafnium and zirconium hydride grades as hydrogen sources for foaming metals and as alloying additions in powder metallurgy
example: Albemarle lists the hafnium hydride grade PS and the zirconium hydride grade PS as hydrogen sources for foaming metals and as alloying constituents in powder metallurgy.
source: albemarle-hfh-ps
where: Applications paragraph
supply:
- subject: Titanium (feedstock for TiH2)
producers:
- country: China
share_percent: 70.3
year: 2025
- country: Japan
share_percent: 14.3
year: 2025
- country: Russia
share_percent: 6.8
year: 2025
- country: Kazakhstan
share_percent: 4.3
year: 2025
- country: Saudi Arabia
share_percent: 3.2
year: 2025
critical_lists:
- list: EU critical raw materials list (titanium metal, as shown on the European Commission page)
listed: true
recycling: 'USGS 2026: consumption data for titanium scrap metal for the titanium metal industry were withheld, because survey responses were limited.'
substitutes: []
source: usgs-mcs2026-titanium
where: 'World Sponge Metal Production table, 2025 column (world total 370,000 t); shares calculated by Space Mushroom from the printed tonnages. Recycling paragraph. Lists: EU page (see sources)'
- subject: Zirconium (feedstock for ZrH2)
producers:
- country: Australia
share_percent: 33.3
year: 2025
- country: South Africa
share_percent: 22.5
year: 2025
- country: Mozambique
share_percent: 13.3
year: 2025
- country: China
share_percent: 8.3
year: 2025
- country: Senegal
share_percent: 5.8
year: 2025
critical_lists:
- list: EU critical raw materials list (zirconium is not in the list printed on the European Commission page)
listed: false
recycling: 'USGS 2026: companies in Oregon and Utah recycled zirconium from new scrap generated during metal production. Refractories are often recycled but could not be quantified.'
substitutes: []
source: usgs-mcs2026-zirconium-hafnium
where: World Mine Production and Reserves table, zirconium mineral concentrates, 2025 column (world total 1,200 thousand t, gross weight); shares calculated by Space Mushroom from the printed tonnages. These are mine shares of concentrate, not sponge metal
- subject: Hafnium (feedstock for HfH2)
producers: []
critical_lists:
- list: EU critical raw materials list (hafnium, as shown on the European Commission page)
listed: true
recycling: 'USGS 2026: hafnium metal recycling was minimal.'
substitutes:
- 'USGS 2026: boron or cadmium-silver-indium alloys can substitute for hafnium metal in nuclear control rods, and zirconium can be used interchangeably with hafnium in certain superalloys.'
source: usgs-mcs2026-zirconium-hafnium
where: Hafnium paragraph of the USGS 2026 summary. The table gives no world primary hafnium production (the USGS text says the data were not available)
media: []
documents:
- title: Sigma-Aldrich safety data sheet, titanium hydride (archived copy hosted by Purdue University)
type: sds
url: https://www.physics.purdue.edu/primelab/safety/MSDS/SDS/titanium%20hydride%20%20-%20Aldrich.pdf
- title: Albemarle technical data sheet, Titanium Hydride, Grade N (issue 2021-07-22)
type: datasheet
url: https://www.albemarle.com/sites/default/files/2025-10/titanium-hydride-grade-n.PDF
year: 2021
- title: Albemarle technical data sheet, Titanium Hydride, Grade G
type: datasheet
url: https://www.albemarle.com/sites/default/files/documents/titanium-hydride-grade-g.PDF
- title: Albemarle technical data sheet, Zirconium Hydride, Grade PS
type: datasheet
url: https://www.albemarle.com/sites/default/files/documents/zirconium-hydride-grade-ps.PDF
- title: Albemarle technical data sheet, Zirconium Hydride, Grade G
type: datasheet
url: https://www.albemarle.com/sites/default/files/documents/zirconium-hydride-grade-g.PDF
- title: Albemarle product page, Hafnium Hydride, Grade PS
type: datasheet
url: https://www.albemarle.com/au/en/product/hafnium-hydride-grade-ps
- title: ATI safety data sheet, SAC050 Zirconium Hydride (EU, Rev 2)
type: sds
url: https://www.atimaterials.com/safety-data-sheets/Documents/EuropeanUnion/EU-EN/SAC/SAC050%20Zirconium%20Hydride%20EU-EN%20Rev2.pdf
- title: ORNL/SPR-2020/1672, Fabrication of Zirconium Hydride with Controlled Hydrogen Loading (Table 1, metal hydride properties)
type: report
url: https://info.ornl.gov/sites/publications/Files/Pub146553.pdf
- title: INL GAIN, High Temperature Moderator Overview (2026 MRP Review), Los Alamos slides
type: report
url: https://gain.inl.gov/content/uploads/4/2026/03/16-Kohnert_HighTemperatureModeratorOverview_2026-MRP-Review.pdf
year: 2026
- title: Pollard et al., Hydrogen desorption kinetics of hafnium hydride powders (Bangor University research output)
type: paper
url: https://research.bangor.ac.uk/en/publications/hydrogen-desorption-kinetics-of-hafnium-hydride-powders/
- title: Zhang et al., The Influence of Titanium Hydride Pretreatment on the Compressive Properties of Aluminum Foam, Materials Science (Medziagotyra) 20(4), 2014
type: paper
url: https://matsc.ktu.lt/index.php/MatSc/article/view/6082/4359
year: 2014
- title: NIST atomic weights and isotopic compositions, Titanium
type: database
url: https://physics.nist.gov/cgi-bin/Compositions/stand_alone.pl?ele=Ti&ascii=html&isotype=some
- title: PubChem compound record, titanium hydride (CID 197094), molecular formula and weight
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/197094
- title: USGS Mineral Commodity Summaries 2026, Titanium and Titanium Dioxide
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-titanium.pdf
year: 2026
- title: USGS Mineral Commodity Summaries 2026, Zirconium and Hafnium
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-zirconium-hafnium.pdf
year: 2026
gaps:
- Hardness, thermal conductivity, thermal expansion and elastic constants of TiH2, ZrH2 and HfH2 were not found in any page read in this run. They are left out.
- 'Melting point of ZrH2 and HfH2: no fetched source. The Albemarle sheets give decomposition, not melting.'
- Crystal structure and space group were not read for TiH2 or ZrH2 in a fetched page, so the identity block has no crystal_system. The HfH2 structure is only in a first-principles paper, which is not used.
- Theoretical density of stoichiometric HfH2 and ZrH2 were not found. The HfH2 value of 11.4 g/cm3 is a commercial powder specification.
- 'Density conflict: TiH2 values are 3.91 g/cm3 (Albemarle, Sigma) and 3.78 g/cm3 (ORNL Table 1). Both are kept, each with its source.'
- Crustal abundance of titanium, zirconium and hafnium was not read in a fetched page in this run, so supply has no abundance entry.
- 'USGS 2025 List of Critical Minerals: the USGS page could not be read in this run. Only the EU list is recorded for titanium, zirconium and hafnium.'
- 'World primary hafnium production: the USGS 2026 summary says the data were not available, so no producer shares are given for hafnium.'
- 'Production route of TiH2, ZrH2 and HfH2 (hydriding of the metal with hydrogen): the ORNL report gives the general method only, so the recipe names the metal and hydrogen without a process temperature.'
- 'Atomic weight of hydrogen: NIST gives the standard atomic weight as the interval [1.00784, 1.00811]. The recipe uses 1.008, which lies inside the interval.'
- 'Ageing under radiation, long-term vacuum storage, and space flight: no source read in this run. The SNAP reactor history is taken from the ORNL introduction only, not from a flight record.'
- 'Hazard statements (H codes) for ZrH2 and HfH2: only the ATI sheet (flammable solids, Category 1, Danger) and the Albemarle handling text were read. American Elements'' H315, H319 and H335 were seen in a search snippet only and are not used.'
- 'Designations (UNS, EN, ASTM and others): no fetched page printed one for these hydrides, so none are listed. The CAS numbers are in identity.cas and in the properties source notes.'
- Hydrogen release curves for TiH2 (the 450 to 560 C and 500 to 670 C pre-treatment figures) were seen in search snippets only and are not used. The 763 K figure is from the KTU paper, which cites Kennedy et al.
- Patent statements on ZrH dissociation pressure at 600 to 800 C in SNAP reactors were seen in search snippets only and are not used.
- 'Property names not in property-canon.yaml: hydrogen_content, hydrogen_density, hydrogen_release_temperature, hydrogen_evolution_onset, hydrogen_desorption_temperature, auto_ignition_temperature, slowing_down_power, moderating_ratio, dissociation_pressure, activation_energy, volume_change and molar_mass. Canonical units are used where the source printed them.'
- 'Environments: no source read supports a space environment tag, so tags.environments is empty.'
sources:
sigma-tih2:
title: Sigma-Aldrich, Safety data sheet for titanium hydride (archived copy hosted by Purdue University)
url: https://www.physics.purdue.edu/primelab/safety/MSDS/SDS/titanium%20hydride%20%20-%20Aldrich.pdf
kind: datasheet
license: supplier safety data sheet, cited not reproduced
albemarle-tih2-n:
title: Albemarle, Titanium Hydride, Grade N, technical data sheet (issue 2021-07-22)
url: https://www.albemarle.com/sites/default/files/2025-10/titanium-hydride-grade-n.PDF
kind: datasheet
year: 2021
license: supplier technical data sheet, cited not reproduced
albemarle-tih2-g:
title: Albemarle, Titanium Hydride, Grade G, technical data sheet
url: https://www.albemarle.com/sites/default/files/documents/titanium-hydride-grade-g.PDF
kind: datasheet
license: supplier technical data sheet, cited not reproduced
albemarle-zrh-ps:
title: Albemarle, Zirconium Hydride, Grade PS, technical data sheet
url: https://www.albemarle.com/sites/default/files/documents/zirconium-hydride-grade-ps.PDF
kind: datasheet
license: supplier technical data sheet, cited not reproduced
albemarle-zrh-g:
title: Albemarle, Zirconium Hydride, Grade G, technical data sheet
url: https://www.albemarle.com/sites/default/files/documents/zirconium-hydride-grade-g.PDF
kind: datasheet
license: supplier technical data sheet, cited not reproduced
albemarle-hfh-ps:
title: Albemarle, Hafnium Hydride, Grade PS, product page with specifications and handling instructions
url: https://www.albemarle.com/au/en/product/hafnium-hydride-grade-ps
kind: datasheet
license: supplier product page, cited not reproduced
ati-zrh-sds:
title: ATI, SAC050 Zirconium Hydride, safety data sheet (EU, Rev 2)
url: https://www.atimaterials.com/safety-data-sheets/Documents/EuropeanUnion/EU-EN/SAC/SAC050%20Zirconium%20Hydride%20EU-EN%20Rev2.pdf
kind: datasheet
license: supplier safety data sheet, cited not reproduced
ornl-zrh-2020:
title: Hu et al., ORNL/SPR-2020/1672, Fabrication of Zirconium Hydride with Controlled Hydrogen Loading (Oak Ridge National Laboratory)
url: https://info.ornl.gov/sites/publications/Files/Pub146553.pdf
kind: report
license: US Department of Energy report
inl-gain-2026:
title: Kohnert, High Temperature Moderator Overview, 2026 MRP Review (INL GAIN, Los Alamos slides)
url: https://gain.inl.gov/content/uploads/4/2026/03/16-Kohnert_HighTemperatureModeratorOverview_2026-MRP-Review.pdf
kind: report
year: 2026
license: DOE GAIN presentation, cited not reproduced
bangor-hfh:
title: Pollard et al., Hydrogen desorption kinetics of hafnium hydride powders (Bangor University research output)
url: https://research.bangor.ac.uk/en/publications/hydrogen-desorption-kinetics-of-hafnium-hydride-powders/
kind: paper
license: journal article, abstract cited not reproduced
ktu-tih2-foam:
title: Zhang et al., The Influence of Titanium Hydride Pretreatment on the Compressive Properties of Aluminum Foam, Materials Science (Medziagotyra) 20(4), 2014, doi 10.5755/j01.ms.20.4.6082
url: https://matsc.ktu.lt/index.php/MatSc/article/view/6082/4359
kind: paper
year: 2014
license: open-access journal article, cited not reproduced
usgs-mcs2026-titanium:
title: USGS Mineral Commodity Summaries 2026, Titanium and Titanium Dioxide
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-titanium.pdf
kind: report
license: public domain (USGS)
usgs-mcs2026-zirconium-hafnium:
title: USGS Mineral Commodity Summaries 2026, Zirconium and Hafnium
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-zirconium-hafnium.pdf
kind: report
license: public domain (USGS)
ec-crm:
title: European Commission, Critical raw materials (list of critical raw materials, including titanium metal and hafnium)
url: https://single-market-economy.ec.europa.eu/sectors/raw-materials/areas-specific-interest/critical-raw-materials_en
kind: web
license: European Commission web page
nist-atomic-weights:
title: NIST, Atomic weights and isotopic compositions for hydrogen, titanium, zirconium and hafnium
url: https://physics.nist.gov/cgi-bin/Compositions/stand_alone.pl?ele=Ti&ascii=html&isotype=some
kind: database
license: NIST public data
pubchem-tih2:
title: PubChem compound record, titanium hydride (CID 197094)
url: https://pubchem.ncbi.nlm.nih.gov/compound/197094
kind: database
license: public domain (NCBI)
license: CC-BY-4.0
updated: '2026-10-26'
review:
status: draft
method: assistant
checked_values: 31
unreachable: 3
caveats: 9
note: 'Written in this run from pages read in this run: the Sigma-Aldrich TiH2 SDS, Albemarle TiH2 grades N and G, Albemarle ZrH grades PS and G, Albemarle HfH2 product page, the ATI ZrH2 SDS, the ORNL ZrH report (Table 1), the INL GAIN moderator slides, the Bangor HfH2 abstract, the KTU TiH2 foaming paper, the USGS 2026 titanium and zirconium-hafnium summaries, the EC critical raw materials page, NIST atomic weights and PubChem CID 197094. Unreachable: USGS 2025 critical minerals page (no readable text), and the NASA NTRS record for the 2021 moderator paper (download failed). Hafnium production and ZrH2 melting point not found.'
story:
recipe:
line: TiH2, ZrH2 and HfH2 each have one metal atom and two hydrogen atoms per formula unit. The metal is bonded to hydrogen in a hydride lattice that expands on hydriding (ORNL). The common preparation is direct reaction of the metal with hydrogen gas, guided by the phase diagram (ORNL); no process temperature for these grades was sourced.
parts:
- name: Titanium
symbol: Ti
atoms: 1
atomic_weight: 47.867
role: Metal in TiH2. NIST gives 47.867 (1).
- name: Zirconium
symbol: Zr
atoms: 1
atomic_weight: 91.224
role: Metal in ZrH2. NIST gives 91.224 (2).
- name: Hafnium
symbol: Hf
atoms: 1
atomic_weight: 178.49
role: Metal in HfH2. NIST gives 178.49 (2).
- name: Hydrogen
symbol: H
atoms: 2
atomic_weight: 1.008
role: Stored in the lattice and released on heating. NIST gives [1.00784, 1.00811] as the standard atomic weight, so 1.008 is used.
risk_groups:
- title: For people
level: 0
verdict: Flammable powder with a dust-explosion risk
lead: The three powders are sold as highly flammable solids with a dust-explosion hazard. The supplier sheets give the handling rules and the fire guidance.
points:
- label: Ignition
line: The Sigma-Aldrich SDS classifies TiH2 as a flammable solid with H228. Keep it away from flames, sparks and heat sources.
- label: Dust
line: Albemarle warns of a dust explosion hazard for TiH2, ZrH2 and HfH2. Avoid dust and provide exhaust ventilation where dust is formed.
- label: Fire
line: Cover a fire only with dry sand, limestone or a class D powder. Do not use water, carbon dioxide or halocarbon.
- title: If a powder or part heats up
lead: These results come from the sources listed, not from incidents.
points:
- label: TiH2
line: The KTU paper gives 763 K as the release temperature for untreated TiH2, and says that pre-treatment at 753 K for 30 min is the most suitable for aluminium foam.
- label: ZrH2
line: ATI says ZrH2 evolves hydrogen above 300 °C. The INL overview gives a 30 atm dissociation pressure for the epsilon phase at 800 °C.
- label: HfH2
line: The Bangor study finds hydrogen release near 350, 415 and 700 °C in three steps.
- title: Handling and storage
points:
- label: Storage
line: Store dry and closed. ZrH2 grade PS is packed dry under argon in tins of at most 5 kg.
- label: Electrostatic discharge
line: Use ground-connected metallic apparatus to avoid sudden ignition by electrostatic discharge (Albemarle).
why: Titanium hydride and its zirconium and hafnium relatives store a large amount of hydrogen in a dense solid. Albemarle sells TiH2 as a reservoir for pure hydrogen, a hydrogen source for foaming metals and an alloying aid in powder metallurgy. ZrH2 has long been the moderator of choice for compact reactors, because it combines a high moderating ratio (55 in ORNL Table 1) with hydrogen density. HfH2 is studied as a moderator and attenuator for compact reactors. The trade is that all three release hydrogen when heated, so their use depends on keeping the hydrogen in place.
uses:
- where: Hydrogen reservoir
line: Albemarle says TiH2 is used as a reservoir for pure hydrogen and yields hydrogen at elevated temperatures in a reversible reaction. The ORNL report describes metal hydrides as a low-risk option for dense hydrogen storage.
- where: Reactor moderators
line: ORNL names the SNAP program and TRIGA reactors as users of zirconium hydride as a moderator. The Bangor abstract calls hafnium hydride a candidate moderator and attenuator for compact reactors.
- where: Foaming and powder metallurgy
line: The KTU paper foams commercially pure aluminium with 1.5 wt% TiH2 to a porosity of about 80 %. Albemarle lists the ZrH2 and HfH2 grades as hydrogen sources for foaming metals and as alloying additions in powder metallurgy.
can_do:
- label: Hydrogen density
benchmark: hydrogen_density
value: '0.152'
line: TiH2 holds 0.152 g of hydrogen per cm3 of hydride, and ZrH2 holds 0.122 g per cm3, both from ORNL Table 1.
- label: Moderation
benchmark: moderating_ratio
value: '55'
line: In ORNL Table 1, ZrH2 has a moderating ratio of 55 against 6.3 for TiH2. The ratio measures slowing-down power against neutron absorption.
- label: Density
benchmark: density
value: '3.91'
line: TiH2 has a density of 3.91 g/cm3 at 20 °C (Albemarle). ZrH2 is 5.6 g/cm3 at 25 °C and HfH2 is 11.4 g/cm3 at 20 °C (Albemarle grades).
compare: The three hydrides are light and dense in hydrogen content, but they differ in density by a factor of about three. TiH2 is the least dense, which suits powder metallurgy. ZrH2 has the highest moderating ratio of the three tabulated in ORNL and it is the moderator in SNAP-type reactors. HfH2 is the densest and releases hydrogen in steps near 350, 415 and 700 °C. The three are compared on density, hydrogen content and hydrogen density because those are the values that all sources give.
compare_rows:
- label: Density
benchmark: density
- label: Hydrogen content
benchmark: hydrogen_content
- label: Hydrogen density
benchmark: hydrogen_density
handling:
- Keep the powder away from flames, sparks and heat. Use ground-connected equipment against electrostatic ignition (Albemarle).
- Avoid dust and use explosion-proof electrical equipment and exhaust ventilation where dust forms (Sigma-Aldrich P241).
- Fight a fire with dry sand, limestone or a class D powder. Do not use water (Albemarle, ATI).
good_for:
- Hydrogen reservoirs and foaming agents, where a dense, stable powder that gives off hydrogen on heating is wanted (Albemarle, KTU).
- Compact-reactor moderators, where ZrH2 has a high moderating ratio (ORNL Table 1) and HfH2 is studied as a moderator and attenuator (Bangor).
watch_out:
- 'Hydrogen loss on heating: TiH2 near 763 K, ZrH2 above 300 °C, and HfH2 in steps near 350, 415 and 700 °C.'
- Dust explosion and flammability. All three are flammable solids and the powder is dangerous in a dust cloud.
- 'The density of TiH2 differs by source: 3.91 g/cm3 from Albemarle and Sigma, and 3.78 g/cm3 in ORNL Table 1.'
verdict: Metal hydride powders are a good hydrogen store and foaming agent, and ZrH2 is a proven reactor moderator. They give off hydrogen on heating and burn as dust, so each use needs the hydrogen kept in place and the powder kept from ignition. Melting, hardness, thermal conductivity and flight data are not sourced here.
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.