Rhenium Re

Re (element, atomic number 75) · CAS 7440-15-5

Rhenium is the element Re, a pure refractory metal with a density of 21.02 g/cm3 and a melting point of 3186 °C.

8 sources · Updated 2026-10-26 · CC BY 4.0

Evidence level

2 of 5

Lab-measured

Stay strong when hot

300 MPa at 1000 °C

Run hot

2200 °C

Heavy metal

21.02 g/cm3

Melting

3186 °C

Thrust gain

20 to 25 s

Recipe, share of the weight

  • Re 100.0%Rhenium

Best for

Structures that must hold strength above 2000 °C: iridium-coated rhenium thrust chambers tested up to about 2200 °C

Weakest at

Oxidation in air or oxygen-rich gas above about 300 °C, which makes uncoated rhenium unusable without a protective coating

Risk at a glance

  • People Low. Powder is flammable
  • If it fails High. Oxidation of uncoated rhenium in hot air or oxygen
  • Corrosion Severe. Uncoated rhenium oxidises to a volatile oxide above about 300 °C, so it needs a protective coating in hot oxygen.

Quick facts: Re

Key properties of Re
PropertyValueBasis
Density21 g/cm³1 sourced value
Yield strength200 to 500 MPa1 sourced value
Tensile strength400 to 700 MPa1 sourced value
Young's modulus460 GPa1 sourced value
Thermal conductivity48 W/(m·K)1 sourced value
Melting point3,186 °C2 sourced values across conditions
Electrical resistivity196 nΩ·m1 sourced value
Maximum service temperature2,200 °C1 sourced value

What is the density of Rhenium (Re)?

Rhenium (Re) has a density of 21 g/cm³. The source and test conditions are listed in the properties table on this page.

What is the thermal conductivity of Rhenium (Re)?

Rhenium (Re) has a thermal conductivity of 48 W/(m·K). The source and test conditions are listed in the properties table on this page.

What is the melting point of Rhenium (Re)?

Rhenium (Re) has a melting point of 3,186 °C. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What is the yield strength of Rhenium (Re)?

Rhenium (Re) has a yield strength of 200 to 500 MPa. The source and test conditions are listed in the properties table on this page.

What is the tensile strength of Rhenium (Re)?

Rhenium (Re) has a tensile strength of 400 to 700 MPa. The source and test conditions are listed in the properties table on this page.

What is Rhenium (Re) used for?

Uses recorded in the sources include Iridium-lined rhenium thrust chamber for a 22 N (5 lbf) bipropellant thruster; Nickel-base superalloy parts for high-temperature turbine engine components; Electrical contacts, thermocouples and electron tubes.

Why it exists

Rhenium is a dense, very high-melting metal: 21.02 g/cm3 and 3186 °C. Its value comes from strength at high temperature. Alloyed into nickel-base superalloys it raises the strength of turbine parts above 1000 °C, and USGS puts that use at about 80 % of 2025 end use. It also forms the structural wall of thrust chambers that NASA-funded tests ran at about 2200 °C. Pure rhenium oxidises in air above about 300 °C, so the flight-candidate chambers carry an iridium coating.

Where it's used

Jet-engine superalloys

Rhenium improves the high-temperature strength of some nickel-base superalloys used in turbine engine parts. USGS estimates superalloys took about 80 % of end use in 2025.

Thruster chambers

A 22 N class NTO/MMH thruster with an iridium-lined rhenium chamber reached 310 s specific impulse in a hot-fire test. NASA lists these chambers for orbit insertion, stationkeeping and attitude control.

Electrical and thermal parts

USGS lists rhenium alloys in electrical contacts, electron tubes, thermocouples and vacuum tubes. Platinum-rhenium catalysts are a further use, about 15 % of 2025 end use.

Recipe

Re (element, atomic number 75); commercial grade 99.99 % (4N) rhenium, Goodfellow

Rhenium is a single-element metal (Re, atomic number 75) (PubChem; Wikipedia). It is mostly recovered as a by-product of roasting molybdenum concentrates from porphyry copper-molybdenum deposits (USGS). Wikipedia states that the metal is made by reducing ammonium perrhenate with hydrogen at high temperature.

What Re is made of
IngredientAtoms per unitShare of the weightWhat it does
Rhenium Re 1 100.0% The whole material. PubChem prints the molecular weight of the element as 186.207.

Weight shares are calculated from standard atomic weights.

What it can do

Stay strong when hot

300 MPa at 1000 °C

measured

Goodfellow gives an approximate tensile strength of 300 MPa at 1000 °C, about 150 MPa at 1500 °C and about 50 MPa at 2500 °C.

Run hot

2200 °C

measured

NASA reports that the iridium-coated rhenium chamber allows thruster operation up to 2200 °C.

Heavy metal

21.02 g/cm3

measured

Density is 21.02 g/cm3 at 20 °C, and the metal is hard, with a Vickers hardness of about 2450 MPa when annealed (Goodfellow).

Melting

3186 °C

measured

The melting point is 3186 °C (3459 K) in both the supplier page and the University of Turku database.

Thrust gain

20 to 25 s

measured

Steady-state firing of the iridium-coated rhenium 22 N engines gave 20 to 25 s higher specific impulse than niobium chambers.

How it compares

Against silicide-coated niobium thrust chambers, the baseline in the NASA reports, iridium-coated rhenium is rated to 2200 °C and gives 20 to 25 s more specific impulse. Rhenium is also costly: USGS gives 2,600 US dollars per kilogram for 99.99 % metal in 2025.

The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.

Benchmarks
MeasurementReWWCHfMoMo-ReMo-30WTZMNbNb alloysW-ReWHAW-CuW-AgWT20VV alloysZrZr alloysTiH2Be
Thermal behavior and safety
Melting pointValue printed on a supplier product page3186 °C3695 Kno data2233 °C2623 °C> 2610 °C2829 °Cno data2477 °C2350 °C3350 °Cno datano datano data3695 K1910 °C1900 °C1852 °C1850 °C> 400 °C1287 °C
Melting point (university database, kelvin as printed)3459 K13695 Kno data2233 °C2623 °C> 2610 °C2829 °Cno data2477 °C2350 °C3350 °Cno datano datano data3695 K1910 °C1900 °C1852 °C1850 °C> 400 °C1287 °C
Thermal conductivity at 25 °CValue printed on a supplier product page48 W/m·K174 W m-1 K-1110 W/(m·K)23 W/(m·K)142 W/(m·K)no datano data130 W/(m·K)53.7 W/(m·K)38.1 W/(m·K)no datano data235 W/(m·K)no data174 W m-1 K-130.7 W/(m·K)no data22 W/(m·K)21.5 W/m-Kno data216 W/(m·K)
Vapour pressure at 2000 °C (custom name, not in property canon)1×10^-7 Pa4no datano datano data1 Pano datano datano datano datano datano datano datano datano datano datano datano datano datano datano data10 kPa
Physical and electrical
Density at 20 °CValue printed on a supplier product page21.02 g/cm³19250 kg/m314.8 g/cm³13.3 g/cm³10.22 g/cm³14.6 g/cm³10.9 g/cm³10.2 g/cm³8.582 g/cm³8.85 g/cm³19.4 g/cm³16.85 to 17.25 g/cc15.15 g/cm³11.75 to 16.1 g/cm³19250 kg m-36.11 g/cm³6.05 g/cm³6.51 g/cm³6.55 g/cc3.91 g/cm³1.85 g/cm³
Electrical resistivity at 20 °CValue printed on a supplier product page196 nΩ·m5.4×10^-8 ohm mno datano data0.056 Ω·mm²/mno datano data0.06 Ω·mm²/mno datano data70 circ mil/ftno data5 µΩ·cm2.3 to 4.6 µΩ·cmno datano datano datano datano datano datano data
Vickers hardness, annealed (custom name, not in property canon)2450 MPa23430 MN m-21350 HV301760 MPano datano datano datano datano datano datano datano datano datano data3430 MN m-2no datano datano datano datano datano data
Other measurements
Boiling pointValue printed on a supplier product page5596 °C5828 Kno data4603 °C4639 °Cno datano datano data4744 °Cno datano datano datano datano data5828 K3407 °Cno datano datano datano data2471 °C
Young's modulusValue printed on a supplier product page460 GPa411 GPa530 to 700 GPa137 GPano datano datano data300 GPa105 GPa90 GPano data340 GPa280 GPano data411 GPa128 GPa125.6 GPa99.2 GPa99.3 GPano data290 GPa
Poisson's ratioValue printed on a supplier product page0.3 -0.28 (no units)no data0.29 -no datano datano datano datano datano datano datano datano datano datano data0.36 -no datano data0.37 -no datano data
Yield strength, annealed to cold-workedRange printed on a supplier product page200 to 500 MPano datano data> 151 MPa265 MPa557 MPano data750 to 900 MPa276 MPa276 MPano data517 MPano datano datano datano data402 MPa321.1 MPa468 MPano data> 207 MPa
Tensile strength, annealed to cold-workedRange printed on a supplier product page400 to 700 MPano datano data> 400 MPa411 MPa719 MPa170 MPa800 to 1000 MPa386 MPa386 MPa220 x 10^3 psi758 MPa620 to 689 MPano datano datano data488 MPa468.1 MPa541 MPano data> 290 MPa
Elongation at break, annealedRange printed on a supplier product page30 to 50 %no datano data> 20 %no data18 %10 %6 to 10 %20 %20 %20 %5 %8.3 %no datano data35 %30.8 %28.9 %28 %no data> 3 %
Tensile strength at 1000 °C (approximate)300 MPa3no datano data> 400 MPa411 MPa719 MPa170 MPa800 to 1000 MPa386 MPa386 MPa220 x 10^3 psi758 MPa620 to 689 MPano datano datano data488 MPa468.1 MPa541 MPano data> 290 MPa
Thrust chamber wall temperature with iridium-coated rhenium, NASA-funded thruster2200 °C5no datano datano datano datano datano data< 825 °Cno datano datano datano datano datano datano datano datano datano datano datano datano data
Specific impulse of 22 N NTO/MMH thruster with iridium-lined rhenium chamber (custom name, not in property canon)310 s6no datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano data
Specific impulse gain over silicide-coated niobium chambers (custom name, not in property canon)20 to 25 s7no datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano data

Why choose it, and why not

Good for

  • Strength above 2000 °C in thrust chambers, tested to 2200 °C with an iridium coating.
  • Superalloy additions that raise high-temperature strength; superalloys took about 80 % of 2025 end use.
  • Recycling: superalloy scrap and spent catalysts are recovered in a closed loop.

Watch out for

  • Oxidation: uncoated rhenium loses material as volatile Re2O7 above about 300 °C in air.
  • Coating life: rhenium diffuses into iridium and eventually causes coating failure, per NASA.
  • Supply: the United States imported about 75 % of its apparent consumption in 2025e, and rhenium was added to the 2025 critical minerals list.
  • Cost: 2,600 US dollars per kilogram for metal in 2025, up 90 % on 2024.
  • No flight result for an iridium-coated rhenium chamber, no thermal expansion value and no radiation data were found for this profile.

Rhenium is a dense, high-melting metal (21.02 g/cm3, 3186 °C) that keeps strength above 2000 °C, which is why it is used in superalloys and in iridium-coated rhenium thrust chambers tested to about 2200 °C. Uncoated, it oxidises above about 300 °C, the iridium coating wears by interdiffusion over time, and the metal is costly. The profile has no UNS designation and no thermal expansion value from a fetched source.

Technical details

For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.

Notes

The method, full conditions and any caveat for the numbered rows above.

Notes for the numbered rows
#MeasurementMethodConditionsCaveat
1Melting point (university database, kelvin as printed)Value printed in a university element database entryform rhenium elementunit in source 3459 K (3186 °C, 5767 °F)—
2Vickers hardness, annealed (custom name, not in property canon)Value printed on a supplier product page; the page also gives Mohs hardness of about 7form annealed rheniumapproximate in source printed as about 2,450 MPa Vickers—
3Tensile strength at 1000 °C (approximate)Approximate value printed in the tensile-at-temperature note on a supplier product pageform rhenium metaltemperature 1000 °Cnote in source printed as about 300 MPa at 1,000 °C—
4Vapour pressure at 2000 °C (custom name, not in property canon)Approximate value printed on a supplier product pageform rhenium metaltemperature 2000 °Cnote in source printed as about 10^-7 Pa—
5Thrust chamber wall temperature with iridium-coated rhenium, NASA-funded thrusterValue stated as the operating temperature the material allows in a NASA technical memorandum abstractsystem iridium-coated rhenium thrust chambertest hot-fire and life tests, NTO/MMH and oxygen/hydrogen propellantsunit in source 2200° C—
6Specific impulse of 22 N NTO/MMH thruster with iridium-lined rhenium chamber (custom name, not in property canon)Measured value printed in a NASA contract final report abstractsystem 22 N (5 lbf) class bipropellant thruster, 150:1 area ratio nozzlepropellant NTO/MMHtest hot-fire test, ground—
7Specific impulse gain over silicide-coated niobium chambers (custom name, not in property canon)Range printed in a NASA technical memorandum abstractsystem 22 N class thrusters, iridium-coated rhenium against niobium chamberstest steady-state firing, ground—

Corrosion and compatibility

What happens when it meets other materials and environments.

Corrosion and compatibility
EnvironmentConcernWhat happens
Air or oxygen-containing gas above about 300 °C severe Uncoated rhenium oxidises to a volatile oxide above about 300 °C, so it needs a protective coating in hot oxygen.1
NTO/MMH rocket combustion gas at 2100 to 2200 °C moderate An iridium coating protects rhenium chambers from hot NTO/MMH combustion gas for at least 15 hours.2
Iridium-coated rhenium at high temperature in vacuum or oxygen moderate Rhenium diffuses into the iridium coating, which will eventually lead to coating failure.3
Corrosion details
#EnvironmentDetailsTest conditions
1 Air or oxygen-containing gas above about 300 °C Goodfellow says rhenium forms volatile Re2O7 above about 300 °C in air. This is why the NASA thrusters use an iridium coating. form pure rhenium metaltemperature above about 300 °Catmosphere air
2 NTO/MMH rocket combustion gas at 2100 to 2200 °C Ultramet's report states that iridium protects rhenium from NTO/MMH combustion gases at 2100 to 2200 °C (3800 to 4000 °F) for at least 15 hours. One iridium-lined rhenium nozzle survived over 4000 cycles and 15 hours of continuous operation with no measurable change in throat dimensions. coating iridium on rhenium, CVDenvironment NTO/MMH combustion gas, 22 N thrustersduration at least 15 hours
3 Iridium-coated rhenium at high temperature in vacuum or oxygen NASA contract report: diffusion of rhenium into iridium will eventually lead to coating failure and subsequent exposure. Above 20 atomic percent rhenium the iridium-rhenium alloy readily oxidised in every environment tested. test diffusion couples held at 4000 °F (2200 °C) in vacuum, and oxidation tests of Ir-Re alloysnote from the NASA Phase II study

Risks and side effects

Hazards to people, what happens when a cell overheats, and how the material is handled and stored.

For people

The opened sources do not describe health effects of rhenium metal. The hazard entries are about the powder and a notification record.

Rhenium as a substance
PubChem lists rhenium as a flammable solid (H228) with the signal word Danger in 63.9 % of the reports that gave codes. Of 393 reports, 137 said it does not meet GHS criteria.
Powder
PubChem says the powdered form is flammable and that no toxicity has been reported in workers handling perrhenic acid or ammonium perrhenate.

If it fails

The failure routes come from NASA ground tests and from the handbook-style property notes, not from flight data.

Hot air
Uncoated rhenium forms volatile Re2O7 above about 300 °C in air, so it must be coated for hot oxygen service.
Coating
NASA reports that rhenium diffuses into the iridium coating, which will eventually cause coating failure.

Handling and storage

Machining
Goodfellow says rhenium needs diamond or CBN grinding wheels. Keep powder away from ignition sources as the PubChem codes advise.

Test details
The original wording and numbers from the sources, for readers who want them.

Failure risks

Failure risks
FailureTrigger and consequence
Oxidation of uncoated rhenium in hot air or oxygenhigh severityUncoated rhenium exposed to air above about 300 °CVolatile Re2O7 forms, so the metal is lost from the surface. Goodfellow gives no rate.
Interdiffusion of rhenium into an iridium coatingmoderate severityIridium-coated rhenium held at high temperature for a long timeThe NASA contract report says the diffusion will eventually lead to coating failure and exposure of the rhenium to combustion gas.
Oxidation of iridium-rhenium alloys with high rhenium contentmoderate severityRhenium above 20 atomic percent in an iridium-rhenium alloyThe alloy readily oxidised in all environments tested, so the coating must stay near pure iridium.

Side effects on surrounding parts

Side effects on surrounding parts
AffectsEffect
Cost of components and of recycling superalloy scrapThe USGS gives a 2025 estimated average price of 2,600 US dollars per kilogram for rhenium metal at 99.99 % purity, a 90 % rise on 2024. Industry sources said recyclers need prices above 3,000 dollars per kilogram to offset processing costs.

Handling and storage

  • Goodfellow says rhenium requires diamond or CBN grinding wheels for machining.
  • The metal powder is flammable (H228 in PubChem). The safety codes are listed in the PubChem record. Handle as a flammable solid in powder form.

Mitigations

  • NASA thrusters use an iridium coating, applied by CVD over a rhenium substrate, to resist oxidation in the combustion gas.

Supply and geography

How common the raw materials are and where they come from.

Rhenium (mine production, rhenium content, 2025)

Top producers (2025)
Chile 37%, China 24.7%, Poland 12.3%, United States 12.1%, Uzbekistan 8.6%
Critical mineral lists
US: listed
Recycling
USGS: nickel-base superalloy scrap and scrapped turbine blades are recycled hydrometallurgically to make rhenium metal for new superalloy melts. Industry sources estimate global secondary production at 20,000 to 25,000 kg in 2025, excluding rhenium recovered in a closed loop from spent catalysts.
Substitutes
USGS: iridium and tin catalysts have been commercially successful in place of platinum-rhenium; cobalt and tungsten for coatings on copper X-ray targets; rhodium and rhodium-iridium for high-temperature thermocouples; tungsten and platinum-ruthenium for electrical contacts; tungsten and tantalum for electron emitters.

Rhenium imports to the United States (rhenium metal, 2021 to 2024)

Top producers (2024)
Chile 38%, Canada 28%, Germany 21%, Poland 11%
Recycling
USGS: United States imports for consumption of unwrought rhenium and powders were 23,000 kg in 2025e, against 12,600 kg in 2024. Net import reliance was 75 % of apparent consumption in 2025e.