Hafnium Hf

Hf (element, atomic number 72) · CAS 7440-58-6

Also known as UNS R02001, ASTM B776, Crystal Bar Hafnium

Hafnium is the element Hf (atomic number 72), a heavy metal with a density of 13.3 g/cm3 that melts at 2233 °C.

8 sources · Updated 2026-10-26 · CC BY 4.0

Evidence level

2 of 5

Lab-measured

Absorb neutrons

104 barns

Carry heat

23.0 W/(m·K)

Weight

13.3 g/cm3

Melting

2233 °C

Strength when annealed

400 MPa

Recipe, share of the weight

  • Hf 100.0%Hafnium

Best for

Absorbing neutrons in reactor control rods (104 barns thermal neutron cross-section) and strengthening nickel superalloys (ATI)

Weakest at

Fine powder and chips, which ignite in air (ATI, ESPI), and strength that depends strongly on oxygen, nitrogen and carbon pickup (ATI)

Risk at a glance

  • People Low. Form-dependent
  • If it fails Severe. Fire in fines and chips
  • Corrosion Severe. Fine hafnium ignites in air, while massive pieces can be worked without burning.

Quick facts: Hf

Key properties of Hf
PropertyValueBasis
Density13.1 to 13.3 g/cm³2 sourced values across conditions
Yield strengthat least 151 MPa1 sourced value
Tensile strengthat least 400 MPa1 sourced value
Young's modulus137 GPa1 sourced value
Thermal conductivity23 W/(m·K)1 sourced value
Thermal expansion (CTE)5.9 ppm/K1 sourced value
Melting point2,233 °C1 sourced value
Specific heat25,690 J/(kg·K)1 sourced value

What is the density of Hafnium (Hf)?

Hafnium (Hf) has a density of 13.1 to 13.3 g/cm³. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What is the thermal conductivity of Hafnium (Hf)?

Hafnium (Hf) has a thermal conductivity of 23 W/(m·K). The source and test conditions are listed in the properties table on this page.

What is the coefficient of thermal expansion of Hafnium (Hf)?

Hafnium (Hf) has a coefficient of thermal expansion of 5.9 ppm/K. The source and test conditions are listed in the properties table on this page.

What is the melting point of Hafnium (Hf)?

Hafnium (Hf) has a melting point of 2,233 °C. The source and test conditions are listed in the properties table on this page.

What is the yield strength of Hafnium (Hf)?

Hafnium (Hf) has a yield strength of at least 151 MPa. The source and test conditions are listed in the properties table on this page.

What are the other names and codes for Hafnium (Hf)?

Hafnium (Hf) is also written as UNS R02001, ASTM B776, Crystal Bar Hafnium. Each code is printed in the source listed beside it in the designations table.

What is Hafnium (Hf) used for?

Uses recorded in the sources include Control rods in nuclear reactors; Nickel-based superalloys for hot-end parts of jet engines; Liquid-rocket thruster nozzles (C103 alloy).

Why it exists

Hafnium is a heavy metal that absorbs neutrons strongly, and that drives its main uses. ATI calls nuclear control rods its biggest application, where its thermal neutron cross-section is 104 barns. In small amounts it strengthens nickel superalloys used in jet engine hot sections. It is also the hafnium share of the C103 niobium alloy used for rocket nozzles, and USGS reports that unwrought hafnium is priced far above zirconium sponge.

Where it's used

Nuclear control rods

ATI calls control rods hafnium's biggest application. A few percent zirconium does not affect its performance there.

Jet engine superalloys

Hafnium strengthens the grain boundaries of nickel superalloys, improving creep ductility and rupture life, in the hot end of jet engines.

Rocket nozzles

The C103 alloy, 89 % niobium, 10 % hafnium and 1 % titanium, is used for liquid-rocket thruster nozzles, including the Apollo Lunar Module engine (Wikipedia).

Recipe

Hf (element, atomic number 72); grades R1 and R3 are unalloyed hafnium, and the alloy-addition product has up to 4.5 % zirconium (ATI)

Hafnium is a single-element metal (Hf) with a hexagonal close-packed structure at room temperature (ATI, Wikipedia). Most of it is made by reducing the tetrachloride with magnesium or sodium, the Kroll process. The iodide (van Arkel) route gives crystal bar with oxygen of 60 ppm or less (PubChem, ATI). ASTM B 776-07 Table 1 sets the impurity limits for each grade, and zirconium must be reported.

What Hf is made of
IngredientAtoms per unitShare of the weightWhat it does
Hafnium Hf 1 100.0% The whole material. Unalloyed grades R1 and R3 are hafnium with a balance; PubChem gives molecular weight 178.49 for the element. Impurity limits are in the risks section.

Weight shares are calculated from standard atomic weights.

What it can do

Absorb neutrons

104 barns

The thermal neutron cross-section is 104 barns (ATI Table 2).

Carry heat

23.0 W/(m·K)

measured

Thermal conductivity is 23.0 W/(m·K) at 298 K (ATI Table 2).

Weight

13.3 g/cm3

measured

Density is 13.3 g/cm3 in ATI's data sheet and 13.1 g/cm3 at 20 °C in the Goodfellow foil sheet.

Melting

2233 °C

measured

Melting point is 2233 °C (ATI). PubChem gives a boiling point of 4603 °C at 760 mmHg.

Strength when annealed

400 MPa

ASTM B 776-07 grade R1 minimums for annealed strip, sheet or plate, longitudinal, at room temperature, are 400 MPa tensile, 151 MPa yield and 20 % elongation.

Stiffness

137 GPa

measured

Young's modulus is 137 GPa at room temperature, with a shear modulus of 54.2 GPa and Poisson's ratio of 0.29 (ATI Table 5).

How it compares

PubChem says the density of zirconium is about half that of hafnium, and ATI says the two metals behave nearly alike in corrosive media. Hafnium and zirconium have nearly opposite nuclear properties, which is why hafnium is the control rod material and zirconium is not. The USGS says zirconium can replace hafnium in certain superalloys. This profile does not carry a zirconium profile, so read the rows as hafnium values only.

The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.

Benchmarks
MeasurementHfWWCMoMo-ReMo-30WTZMNbNb alloysReW-ReWHAW-CuW-AgWT20VV alloysZrZr alloysTiH2Be
Thermal behavior and safety
Melting point, hafnium2233 °C33695 Kno data2623 °C> 2610 °C2829 °Cno data2477 °C2350 °C3186 °C3350 °Cno datano datano data3695 K1910 °C1900 °C1852 °C1850 °C> 400 °C1287 °C
Thermal conductivity, hafnium23 W/(m·K)5174 W m-1 K-1110 W/(m·K)142 W/(m·K)no datano data130 W/(m·K)53.7 W/(m·K)38.1 W/(m·K)48 W/m·Kno datano data235 W/(m·K)no data174 W m-1 K-130.7 W/(m·K)no data22 W/(m·K)21.5 W/m-Kno data216 W/(m·K)
Specific heat capacity, hafnium25.69 J/(g·K)6no datano data0.25 J/(g·K)no datano data0.25 J/(g·K)264.8 J/(kg·K)no datano datano datano datano datano datano datano datano data0.2847 kJ/(kg·K)0.285 J/g-°Cno data1.95 J/g/°C
Thermal neutron cross-section, hafnium104 barn17no datano datano datano datano datano datano datano datano datano datano datano datano datano datano datano data0.18 barns0.22 barnsno datano data
Physical and electrical
Density, hafnium alloy-addition data sheet13.3 g/cm³119250 kg/m314.8 g/cm³10.22 g/cm³14.6 g/cm³10.9 g/cm³10.2 g/cm³8.582 g/cm³8.85 g/cm³21.02 g/cm³19.4 g/cm³16.85 to 17.25 g/cc15.15 g/cm³11.75 to 16.1 g/cm³19250 kg m-36.11 g/cm³6.05 g/cm³6.51 g/cm³6.55 g/cc3.91 g/cm³1.85 g/cm³
Density, hafnium foil (Goodfellow)Value printed in a supplier product datasheet13.1 g/cm³219250 kg/m314.8 g/cm³10.22 g/cm³14.6 g/cm³10.9 g/cm³10.2 g/cm³8.582 g/cm³8.85 g/cm³21.02 g/cm³19.4 g/cm³16.85 to 17.25 g/cc15.15 g/cm³11.75 to 16.1 g/cm³19250 kg m-36.11 g/cm³6.05 g/cm³6.51 g/cm³6.55 g/cc3.91 g/cm³1.85 g/cm³
Vickers hardness, hafnium1760 MPa163430 MN m-21350 HV30no datano datano datano datano datano data2450 MPano datano datano datano data3430 MN m-2no datano datano datano datano datano data
Other measurements
Boiling point, hafnium4603 °C45828 Kno data4639 °Cno datano datano data4744 °Cno data5596 °Cno datano datano datano data5828 K3407 °Cno datano datano datano data2471 °C
Coefficient of thermal expansion, hafnium5.9 ppm/K74.5×10^-6 K-15.5 μm/(m·K)5.2 ppm/Kno datano data5.3 to 5.7 ppm/K7.07 ppm/Kno datano datano datano data8.3 ppm/Kno datano data8.3 ppm/Kno data6.3 10-6/°C6 µm/(m·°C)no data11.3 ppm/°C
Young's modulus, hafnium at room temperature137 GPa8411 GPa530 to 700 GPano datano datano data300 GPa105 GPa90 GPa460 GPano data340 GPa280 GPano data411 GPa128 GPa125.6 GPa99.2 GPa99.3 GPano data290 GPa
Shear modulus, hafnium at room temperature54.2 GPa9161 GPano datano datano datano datano datano datano datano datano datano datano datano datano datano datano data36.2 GPa36.2 GPano datano data
Poisson's ratio, hafnium0.29 -100.28 (no units)no datano datano datano datano datano datano data0.3 -no datano datano datano datano data0.36 -no datano data0.37 -no datano data
Tensile strength, annealed, longitudinal, room temperature, grade R1> 400 MPa11no datano data411 MPa719 MPa170 MPa800 to 1000 MPa386 MPa386 MPa400 to 700 MPa220 x 10^3 psi758 MPa620 to 689 MPano datano datano data488 MPa468.1 MPa541 MPano data> 290 MPa
Yield strength Rp0.2, annealed, longitudinal, room temperature, grade R1> 151 MPa12no datano data265 MPa557 MPano data750 to 900 MPa276 MPa276 MPa200 to 500 MPano data517 MPano datano datano datano data402 MPa321.1 MPa468 MPano data> 207 MPa
Elongation, annealed, longitudinal, room temperature, grade R1> 20 %13no datano datano data18 %10 %6 to 10 %20 %20 %30 to 50 %20 %5 %8.3 %no datano data35 %30.8 %28.9 %28 %no data> 3 %
Tensile strength, annealed, longitudinal, 315 °C, grade R1> 172 MPa14no datano data411 MPa719 MPa170 MPa800 to 1000 MPa386 MPa386 MPa400 to 700 MPa220 x 10^3 psi758 MPa620 to 689 MPano datano datano data488 MPa468.1 MPa541 MPano data> 290 MPa
Yield strength Rp0.2, annealed, longitudinal, 315 °C, grade R1> 76 MPa15no datano data265 MPa557 MPano data750 to 900 MPa276 MPa276 MPa200 to 500 MPano data517 MPano datano datano datano data402 MPa321.1 MPa468 MPano data> 207 MPa

Why choose it, and why not

Good for

  • Neutron absorption: 104 barns thermal neutron cross-section in control rods (ATI).
  • Superalloy additive: strengthens nickel superalloy grain boundaries and improves creep ductility (ATI).
  • Rocket nozzles: the C103 alloy with 10 % hafnium, used in liquid-rocket thrusters (Wikipedia).

Watch out for

  • Fine powder and chips ignite in air, and water on burning fines can cause a violent explosion (ATI, ESPI).
  • Strength and ductility depend strongly on oxygen, nitrogen and carbon (ATI).
  • Supply data are thin: USGS gives no world production figures, and the 2021 to 2024 import shares are Germany 54 %, China 21 % and France 12 %.
  • The foil and the powder carry different hazard classifications in the sources.

Hafnium is a neutron absorber and a superalloy additive, with a density of 13.3 g/cm3 and a melting point of 2233 °C. Its strong neutron capture and high melting point are well documented, but its room-temperature strength is only a minimum from one standard, and its supply data are incomplete. Fine powder is pyrophoric, so fines need the handling steps above. The only rocket use read is the Apollo Lunar Module nozzle in C103 alloy.

Technical details

For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.

Other names and standards

The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.

Other names and standards
SystemCodes
UNSR02001 (alloy-addition hafnium with zirconium up to 4.5 %)
ASTMB776 (strip, sheet and plate, grades R1 and R3)
Trade nameCrystal Bar Hafnium (iodide crystal bar form)

Notes

The method, full conditions and any caveat for the numbered rows above.

Notes for the numbered rows
#MeasurementMethodConditionsCaveat
1Density, hafnium alloy-addition data sheetTypical value printed in a manufacturer technical data sheet, which says the data are typical and not maximum or minimum valuestemperature not stated in the tableunit in source 13.3 g/cm3 (0.481 lbs / in3)—
2Density, hafnium foil (Goodfellow)—temperature 20 °Cform hafnium foilThe same supplier page gives melting point 2227 and a different density from ATI's 13.3, so the sources differ by about 0.2 g/cm3.
3Melting point, hafniumValue printed in a manufacturer technical data sheetunit in source 2233°C (4051°F)pressure not stated—
4Boiling point, hafniumValue printed in the Wikipedia infobox; PubChem's Experimental Properties also list 4603 °C at 760 mmHgpressure not stated in the infoboxunit in source 4876 K (4603 °C, 8317 °F)ATI prints 4690 °C in its data sheet, and PubChem gives 4602 °C in one entry. The sources differ by about 90 °C, so this profile records the Wikipedia infobox value.
5Thermal conductivity, hafniumValue printed in a manufacturer technical data sheettemperature 298 Kunit in source 23.0 W/m • K @298K—
6Specific heat capacity, hafniumValue printed in a manufacturer technical data sheettemperature not stated in the tableunit in source 25.69 J/g • K—
7Coefficient of thermal expansion, hafniumValue printed in a manufacturer technical data sheet; 10-6 m/m per K is the same unit as ppm/Ktemperature not stated in the tableunit in source 5.9 X 10-6 m/m • K-1—
8Young's modulus, hafnium at room temperatureValue printed in a manufacturer technical data sheet, typical valuestemperature room temperatureform not statedGoodfellow's foil page prints a tensile modulus of 141 GPa, close to ATI's 137 GPa. American Elements prints 78 GPa as a theoretical value, which was not opened.
9Shear modulus, hafnium at room temperatureValue printed in a manufacturer technical data sheet, typical valuestemperature room temperature—
10Poisson's ratio, hafniumValue printed in a manufacturer technical data sheettemperature not stated in the table—
11Tensile strength, annealed, longitudinal, room temperature, grade R1Minimum value printed in the mechanical property table of ASTM B 776-07grade R1 (nuclear)temper annealeddirection longitudinaltemperature room temperatureunit in source 58 ksi (400 MPa)product form strip, sheet and plate (ASTM B 776-07 Table 3)ATI's data sheet gives the same 400 MPa minimum for rod and plate in the longitudinal direction.
12Yield strength Rp0.2, annealed, longitudinal, room temperature, grade R1Minimum value printed in the mechanical property table of ASTM B 776-07grade R1 (nuclear)temper annealeddirection longitudinaltemperature room temperatureunit in source 22 ksi (151 MPa)product form strip, sheet and plate (ASTM B 776-07 Table 3)ATI prints 150 MPa for the same minimum yield strength in its rod and plate table, and this profile records the ASTM value.
13Elongation, annealed, longitudinal, room temperature, grade R1Minimum value printed in the mechanical property table of ASTM B 776-07grade R1 (nuclear)temper annealeddirection longitudinaltemperature room temperaturegauge length 2 in. (50 mm)ATI prints a typical 25 to 30 % elongation at room temperature, dependent on purity, which is a different basis and is not used.
14Tensile strength, annealed, longitudinal, 315 °C, grade R1Minimum value printed in the mechanical property table of ASTM B 776-07grade R1 (nuclear)temper annealeddirection longitudinaltemperature 315 °C (600 °F)unit in source 25 ksi (172 MPa)—
15Yield strength Rp0.2, annealed, longitudinal, 315 °C, grade R1Minimum value printed in the mechanical property table of ASTM B 776-07grade R1 (nuclear)temper annealeddirection longitudinaltemperature 315 °C (600 °F)unit in source 11 ksi (76 MPa)—
16Vickers hardness, hafniumValue printed in a manufacturer technical data sheet; the unit is printed as MPatemperature not stated in the tableunit in source 1760 MPaNo canonical name exists for hardness in the property file, so vickers_hardness is a new name and is listed in gaps.
17Thermal neutron cross-section, hafniumValue printed in a manufacturer technical data sheetneutron thermalunit in source 104 BarnsNo canonical name exists for this property in the property file, so thermal_neutron_cross_section is a new name and is listed in gaps.

Corrosion and compatibility

What happens when it meets other materials and environments.

Corrosion and compatibility
EnvironmentConcernWhat happens
Hot water at 360 °C and 18.5 MPa low Grade R1 hafnium may gain no more than 10 mg/dm2 in 672 h of 360 °C water.1
Mineral acids, alkalis and hydrogen fluoride moderate Hafnium resists nitric acid and dilute hydrochloric or sulfuric acid, but fluoride traces make mineral acids attack it.2
Hydrogen at about 700 °C moderate Hafnium absorbs hydrogen quickly at 700 °C, forming HfH.3
Fine powder and chips in air or water severe Fine hafnium ignites in air, while massive pieces can be worked without burning.4
Corrosion details
#EnvironmentDetailsTest conditions
1 Hot water at 360 °C and 18.5 MPa ASTM B 776 specifies a test in water at 680 °F (360 °C) and 2690 psi (18.5 MPa) for 672 h. Grade R1 coupons must show a weight gain of not more than 10 mg/dm2. Grade R3 is tested for information only. specimen two random samples from each lotduration 672 htemperature 360 °C (680 °F)pressure 18.5 MPa (2690 psi)grade R1 (nuclear)
2 Mineral acids, alkalis and hydrogen fluoride PubChem summarises that hafnium is unaffected by nitric acid in all concentrations, resists dilute hydrochloric and sulfuric acid, is attacked by all mineral acids if traces of fluoride are present, is slowly attacked by concentrated sulfuric acid, and is very resistant to alkalis. It is soluble in hydrogen fluoride. ATI says its corrosion behaviour is very similar to zirconium. temperature not stated
3 Hydrogen at about 700 °C PubChem records that hafnium rapidly absorbs hydrogen to form HfH at 700 °C. ATI notes that mechanical properties are strongly affected by interstitial contamination. temperature 700 °Catmosphere hydrogen
4 Fine powder and chips in air or water ATI says massive pieces can be heated and worked without burning, but sponge, fines, machine chips and foil can easily ignite and burn at very high temperature. ESPI says solid hafnium will not ignite and 10 micron powder may autoignite at room temperature. form powder, chips, turnings, sponge and foilparticle size 10 micron powder (ESPI)

Risks and side effects

Hazards to people, what happens when a cell overheats, and how the material is handled and stored.

For people

The hazard is in the fine form. Solid hafnium has no known toxicity, but fine powder and chips can catch fire, and the sources disagree on the classification.

Powder and chips
PubChem lists H250, catches fire spontaneously if exposed to air, with signal word Danger, for the notifications it reports (50.6 % of reports). A 1996 supplier sheet says solid hafnium will not ignite, but 10 micron powder may autoignite at room temperature.
Foil
A 2022 Stanford Advanced Materials sheet does not classify hafnium foil under CLP, which differs from the H250 entry for the powder.
Dust
The OSHA and NIOSH exposure limit is 0.5 mg/m3 as a time-weighted average.

If it fails

The sources give three failure routes: a fire in fines, loss of ductility from interstitial gases, and weight gain above the grade limit in hot water.

Fire in fines
ATI says fines and chips ignite easily and burn at very high temperature, and ESPI warns that water on burning fines can cause a violent explosion.
Gas pickup
ATI says mechanical properties depend strongly on interstitial contamination. PubChem says hafnium rapidly absorbs hydrogen at 700 °C to form HfH.
Hot water
ASTM B 776-07 allows grade R1 a weight gain of no more than 10 mg/dm2 after 672 h in 360 °C water at 18.5 MPa.

Handling and storage

Keep fines wet or dry
ATI says to keep chips covered with water and never let it dry out. ESPI says wet fines need more than 25 % water by weight.
Fire
Use salt, sand, metal or a Type D extinguisher on small fires. Never use water or CO2 (ATI).

Test details
The original wording and numbers from the sources, for readers who want them.

Failure risks

Failure risks
FailureTrigger and consequence
Fire in fines and chipscritical severityFinely divided hafnium such as powder, chips, turnings or sponge exposed to air or to waterFines ignite and burn at extremely high temperatures (ATI). ESPI warns that water on burning fines can cause a violent explosion, and that hydrogen and steam from a wet mass can explode. Water and CO2 feed such fires (ATI).
Loss of ductility from interstitial gasesmoderate severityPickup of oxygen, nitrogen or carbon during melting, processing or serviceATI says mechanical properties are strongly affected by interstitial contamination, and that a very low interstitial content may be needed for ductility. Crystal bar is made with oxygen of 60 ppm or less for critical applications.
Hydrogen pickup at high temperaturemoderate severityHafnium exposed to hydrogen at about 700 °CHafnium rapidly absorbs hydrogen to form HfH (PubChem). The source gives no embrittlement value.
Corrosion above the grade R1 limit in hot waterlow severityExposure to 360 °C water at 18.5 MPa for 672 hA weight gain above 10 mg/dm2 fails the grade R1 corrosion requirement in ASTM B 776-07.

Side effects on surrounding parts

Side effects on surrounding parts
AffectsEffect
Purity and grade of hafnium metalHafnium is hard to separate from zirconium. PubChem says zirconium and hafnium are two of the most difficult elements to separate, and that very pure hafnium has been made with zirconium as the main impurity.

Handling and storage

  • Specify the grade, because the limits differ. Grade R1 (nuclear) maximum oxygen 0.040, nitrogen 0.010 and iron 0.050 weight %; grade R3 (commercial) oxygen 0.130, nitrogen 0.015 and iron 0.0750 weight %, with zirconium reported (ASTM B 776-07 Table 1).
  • Keep chips and fines covered with water, or in nonflammable containers in isolated areas. The water must not be allowed to evaporate or the material to dry out (ATI).
  • Keep fine turnings completely dry or very wet. If wet, the water content should be more than 25 % by weight, and do not accumulate large quantities of fines (ESPI).
  • Fight small fires with salt, sand, metal or a Type D extinguisher. Never use water or CO2 (ATI).

Supply and geography

How common the raw materials are and where they come from.

Hafnium abundance

3.0 to 4.8 ppm of Earth's upper crust by mass, occurring mainly in zircon, where 1 to 4 % of the zirconium is replaced by hafnium (Wikipedia)

Hafnium metal (U.S. imports of unwrought hafnium, import shares 2021 to 2024)

Top producers (2024)
Germany 54%, China 21%, France 12%, United Kingdom 8%
Recycling
USGS: hafnium metal recycling was minimal. Two companies in Oregon and Utah produced zirconium and hafnium metal from zirconium intermediates in 2025.
Substitutes
USGS: boron or cadmium-silver-indium alloys can substitute for hafnium metal in nuclear control rods, and zirconium can be used interchangeably with hafnium in certain superalloys. Niobium, stainless steel and tantalum give some substitution in nuclear applications.