Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30) PBT-GF30

(C12H12O4)n repeat unit for the polybutylene terephthalate matrix, filled with 30% glass fibre by weight · CAS 24968-12-5

Also known as TECADUR PBT GF30 natural, TECADUR PBT GF30, PRECITE® P3 GF 30 natural, PBT GF30

Polybutylene terephthalate reinforced with 30% glass fibre (PBT-GF30) is a stiff, dimensionally stable polyester for moulded electrical and precision parts.

11 sources · Updated 2026-11-01 · CC BY 4.0

Evidence level

2 of 5

Lab-measured

Stiff under load

3400 MPa

Hold its shape with heat

205 °C

Keep strength when hot and wet

145 MPa

Recipe, share of the weight

  • balancePolybutylene terephthalate matrix
  • 30%Glass fibre
  • C not statedCarbon
  • H not statedHydrogen
  • O not statedOxygen

Best for

Stiff, dimensionally stable moulded and machined parts for electrical and precision uses that stay dry: Akro prints a flexural modulus of 10500 MPa and a heat deflection temperature of 205 °C at 1.8 MPa

Weakest at

Heat and water: Borges et al. 2021 measured 44 MPa tensile strength at 130 °C on specimens dry as supplied, and an equilibrium water uptake of 0.56 % at 130 °C

Risk at a glance

  • People Low. Not classified in the safety sheet read
  • If it fails High. Thermal decomposition at high temperature
  • Corrosion Moderate. PBT is sensitive to hot water above 60 °C, according to Wikipedia.

Quick facts: PBT-GF30

Key properties of PBT-GF30
PropertyValueBasis
Density1.46 to 1.53 g/cm³3 sourced values across conditions
Yield strength46 MPa1 sourced value
Tensile strength112 to 145 MPa2 sourced values across conditions
Young's modulus3.4 to 10 GPa3 sourced values across conditions
Thermal conductivity0.33 W/(k*m)1 sourced value
Melting point220 to 230 °C3 sourced values across conditions
Specific heat1,200 J/(kg·K)1 sourced value
Maximum service temperature110 to 200 °C2 sourced values across conditions

What is the density of Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30)?

Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30) has a density of 1.46 to 1.53 g/cm³. The range covers 3 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What is the thermal conductivity of Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30)?

Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30) has a thermal conductivity of 0.33 W/(k*m). The source and test conditions are listed in the properties table on this page.

What is the melting point of Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30)?

Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30) has a melting point of 220 to 230 °C. The range covers 3 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What is the yield strength of Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30)?

Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30) has a yield strength of 46 MPa. The source and test conditions are listed in the properties table on this page.

What is the tensile strength of Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30)?

Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30) has a tensile strength of 112 to 145 MPa. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.

What are the other names and codes for Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30)?

Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30) is also written as TECADUR PBT GF30 natural, TECADUR PBT GF30, PRECITE® P3 GF 30 natural, PBT GF30. Each code is printed in the source listed beside it in the designations table.

What is Polybutylene terephthalate, 30% glass fibre reinforced (PBT-GF30) used for?

Uses recorded in the sources include Electrical and precision moulded parts; Dimensionally stable moulded and machined engineering parts.

Why it exists

Polybutylene terephthalate with 30% glass fibre (PBT-GF30) is a stiff, dimensionally stable moulded polymer. Ensinger's TECADUR PBT GF30 natural prints a tensile modulus of 3400 MPa and a melting temperature of 224 °C. Akro's PRECITE P3 GF 30 natural (6850) prints a tensile modulus of 10000 MPa, a heat deflection temperature of 205 °C at 1.8 MPa, and a density of 1.53 g/cm³. The two datasheets disagree, so both values are shown.

Recipe

(C12H12O4)n repeat unit for the polybutylene terephthalate matrix, filled with 30% glass fibre by weight

Polybutylene terephthalate is made by polymerising 1,4-butanediol with terephthalic acid, and its repeat unit is C12H12O4 (Wikipedia). This grade is a PBT matrix filled with 30% glass fibre by weight (Ensinger). Wikipedia states that a size is applied to glass fibre after drawing in the continuous filament process, to protect the fibre and to give it affinity for a resin.

What PBT-GF30 is made of
IngredientShare of the weightWhat it does
Polybutylene terephthalate matrix balance Semicrystalline polyester matrix, repeat unit C12H12O4
Glass fibre 30% Reinforcing filler at 30% by weight in this grade
Carbon C not stated Carbon atoms in the PBT repeat unit C12H12O4
Hydrogen H not stated Hydrogen atoms in the PBT repeat unit C12H12O4
Oxygen O not stated Oxygen atoms in the PBT repeat unit C12H12O4

Weight shares are as printed in the sources.

What it can do

Stiff under load

3400 MPa

measured

Akro prints a flexural modulus of 10500 MPa and a flexural strength of 230 MPa for PRECITE P3 GF 30 natural (6850), both per ISO 178 at 2 mm/min.

Hold its shape with heat

205 °C

measured

Akro prints a heat deflection temperature (HDT/A) of 205 °C at 1.8 MPa for the same grade, per ISO 75.

Keep strength when hot and wet

145 MPa

measured

Borges et al. measured 44 MPa tensile strength at 130 °C on specimens dry as supplied, and 0.56 % equilibrium water uptake at 130 °C, for a PBT-GF30 whose grade they do not name.

How it compares

Two datasheets for the same 30% glass-fibre PBT disagree. Ensinger prints a tensile modulus of 3400 MPa in a DIN EN ISO 527-2 test and a density of 1.46 g/cm3 with no test standard, while Akro prints 10000 MPa per ISO 527-2 and a density of 1.53 g/cm³ per ISO 1183. Borges et al. report 8.6 GPa at room temperature for a PBT-GF30 whose grade is not named. Read the rows as values for different grades and test methods, not as a ranking.

The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Compare every grade in the family.

Benchmarks
MeasurementPBT-GF30
Thermal behavior and safety
Melting temperature (Ensinger)224 °C9
Thermal conductivity (Ensinger)0.33 W/(k*m)10
Specific heat (Ensinger)1.2 J/(g*K)11
Heat deflection temperature, HDT/A (Akro)205 °C24
Melting temperature (Akro)225 °C25
Melting point, safety information range (tbgroup)220 to 230 °C43
Thermal decomposition onset (tbgroup)> 290 °C46
Lifetime and stability
Melt volume rate (Akro)9 cm³/10 min31
Physical and electrical
Density (Ensinger)1.46 g/cm³14
Density (Akro)1.53 g/cm³26
Density, safety information range (tbgroup)1.3 to 1.8 g/ccm42
Temperature behavior
Glass transition temperature (Borges et al.)49 °C41
Other measurements
Modulus of elasticity, tensile test (Ensinger)3400 MPa1
Tensile strength at yield (Ensinger)46 MPa2
Elongation at yield (Ensinger)5 %3
Elongation at break (Ensinger)6 %4
Flexural strength (Ensinger)78 MPa5
Modulus of elasticity, flexural test (Ensinger)3400 MPa6
Compression modulus (Ensinger)2800 MPa7
Charpy impact strength (Ensinger)37 kJ/m28
Service temperature, short term (Ensinger)200 °C12
Service temperature, long term (Ensinger)110 °C13
Water absorption after 24 h (Ensinger)0.02 %15
Water absorption after 96 h (Ensinger)0.04 %16
Tensile modulus (Akro)10000 MPa17
Tensile stress at break (Akro)145 MPa18
Tensile strain at break (Akro)3 %19
Flexural modulus (Akro)10500 MPa20
Flexural strength (Akro)230 MPa21
Charpy impact strength (Akro)65 kJ/m222
Charpy notched impact strength (Akro)11 kJ/m223
Humidity absorption (Akro)0.2 %27
Moulding shrinkage, flow direction (Akro)0.3 %28
Moulding shrinkage, transverse direction (Akro)0.9 %29
Comparative tracking index (Akro)350 V30
Equilibrium water uptake at 35 °C (Borges et al.)0.47 %32
Equilibrium water uptake at 70 °C (Borges et al.)0.5 %33
Equilibrium water uptake at 130 °C (Borges et al.)0.56 %34
Young's modulus, room temperature, standard specimens (Borges et al.)8.6 GPa35
Tensile strength, room temperature, standard specimens (Borges et al.)112 MPa36
Young's modulus at 70 °C (Borges et al.)4.6 GPa37
Tensile strength at 70 °C (Borges et al.)66 MPa38
Young's modulus at 130 °C (Borges et al.)2.3 GPa39
Tensile strength at 130 °C (Borges et al.)44 MPa40
Flash point (tbgroup)> 400 °C44
Ignition point (tbgroup)> 350 °C45

Why choose it, and why not

Good for

  • Stiff moulded parts: Akro prints a flexural modulus of 10500 MPa for PRECITE P3 GF 30 natural (6850).
  • Dimensionally stable parts: Akro prints moulding shrinkage of 0.3 % (flow) and 0.9 % (transverse) per ISO 294-4.
  • Electrical parts that stay dry: Akro prints a comparative tracking index of 350 V per IEC 60112 and a low water absorption.

Watch out for

  • Water: Borges et al. measured 0.47 % equilibrium uptake at 35 °C, rising to 0.56 % at 130 °C, and report that the tensile values after water ageing are only in a figure.
  • Heat: the tensile strength falls to 66 MPa at 70 °C and 44 MPa at 130 °C on dry specimens, against 112 MPa at room temperature.
  • Thermal decomposition starts above 290 °C and releases toxic gases, including traces of hydrogen cyanide.
  • No outgassing, radiation or atomic oxygen data for this grade was found, so no space behaviour is recorded.

PBT-GF30 is a stiff moulded polymer with a flexural modulus of 10500 MPa and a heat deflection temperature of 205 °C at 1.8 MPa in the Akro grade read. The Ensinger grade reads 3400 MPa tensile modulus, so the two datasheets differ. Its weak point is hot water: Borges et al. report 0.56 % equilibrium water uptake at 130 °C and 44 MPa tensile strength at 130 °C.

Technical details

For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.

Other names and standards

The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.

Other names and standards
SystemCodes
Trade nameTECADUR PBT GF30 natural, TECADUR PBT GF30, PRECITE® P3 GF 30 natural, PBT GF30

Notes

The method, full conditions and any caveat for the numbered rows above.

Notes for the numbered rows
#MeasurementMethodConditionsCaveat
1Modulus of elasticity, tensile test (Ensinger)Typical value printed on the manufacturer product pagegrade TECADUR PBT GF30 naturaltest speed 1 mm/minstandard DIN EN ISO 527-2—
2Tensile strength at yield (Ensinger)Typical value printed on the manufacturer product pagegrade TECADUR PBT GF30 naturaltest speed 50 mm/minstandard DIN EN ISO 527-2—
3Elongation at yield (Ensinger)Typical value printed on the manufacturer product pagegrade TECADUR PBT GF30 naturaltest speed 50 mm/minstandard DIN EN ISO 527-2point at yield—
4Elongation at break (Ensinger)Typical value printed on the manufacturer product pagegrade TECADUR PBT GF30 naturaltest speed 50 mm/minstandard DIN EN ISO 527-2point at break—
5Flexural strength (Ensinger)Typical value printed on the manufacturer product pagegrade TECADUR PBT GF30 naturaltest speed 2 mm/minload 10 Nstandard DIN EN ISO 178—
6Modulus of elasticity, flexural test (Ensinger)Typical value printed on the manufacturer product pagegrade TECADUR PBT GF30 naturaltest speed 2 mm/minload 10 Nstandard DIN EN ISO 178—
7Compression modulus (Ensinger)Typical value printed on the manufacturer product pagegrade TECADUR PBT GF30 naturaltest speed 5 mm/minload 10 Nstandard EN ISO 604—
8Charpy impact strength (Ensinger)Typical value printed on the manufacturer product pagegrade TECADUR PBT GF30 naturalstandard DIN EN ISO 179-1eUnotch unnotched (eU)note printed max. 7,5J—
9Melting temperature (Ensinger)Typical value printed on the manufacturer product pagegrade TECADUR PBT GF30 naturalstandard DIN EN ISO 11357unit as printed C—
10Thermal conductivity (Ensinger)Typical value printed on the manufacturer product page; the page cites ISO 22007-4:2008 as the methodgrade TECADUR PBT GF30 naturalunit as printed W/(k*m)—
11Specific heat (Ensinger)Typical value printed on the manufacturer product page; the page cites ISO 22007-4:2008 as the methodgrade TECADUR PBT GF30 naturalunit as printed J/(g*K)—
12Service temperature, short term (Ensinger)Typical value printed on the manufacturer product page; the page gives no test standardgrade TECADUR PBT GF30 naturalduration short term—
13Service temperature, long term (Ensinger)Typical value printed on the manufacturer product page; the page gives no test standardgrade TECADUR PBT GF30 naturalduration long term—
14Density (Ensinger)Value printed in the Facts section of the manufacturer product page; no test standard printedgrade TECADUR PBT GF30 naturaltemperature not printed—
15Water absorption after 24 h (Ensinger)Typical value printed on the manufacturer product page; standard DIN EN ISO 62 printedgrade TECADUR PBT GF30 naturaltime 24 htemperature 23 °C—
16Water absorption after 96 h (Ensinger)Typical value printed on the manufacturer product page; standard DIN EN ISO 62 printedgrade TECADUR PBT GF30 naturaltime 96 htemperature 23 °C—
17Tensile modulus (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)test speed 1 mm/mincondition printed d.a.m.standard ISO 527-2—
18Tensile stress at break (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)test speed 5 mm/mincondition printed d.a.m.standard ISO 527-2—
19Tensile strain at break (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)test speed 5 mm/mincondition printed d.a.m.standard ISO 527-2point at break—
20Flexural modulus (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)test speed 2 mm/mincondition printed d.a.m.standard ISO 178—
21Flexural strength (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)test speed 2 mm/mincondition printed d.a.m.standard ISO 178—
22Charpy impact strength (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)standard ISO 179-1/1eUtemperature 23 °Ccondition printed d.a.m.—
23Charpy notched impact strength (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)standard ISO 179-1/1eAtemperature 23 °Ccondition printed d.a.m.—
24Heat deflection temperature, HDT/A (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)load 1.8 MPastandard ISO 75 (HDT/A)—
25Melting temperature (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)standard ISO 11357-3method printed DSC, 10 K/min—
26Density (Akro)Typical value printed on the manufacturer product page, with the ISO 1183 standard printedgrade PRECITE P3 GF 30 natural (6850)standard ISO 1183temperature 23 °Cprinted form 1,53 g/cm³—
27Humidity absorption (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)standard ISO 1110temperature 70 °Crelative humidity 62 %—
28Moulding shrinkage, flow direction (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)standard ISO 294-4direction flow—
29Moulding shrinkage, transverse direction (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)standard ISO 294-4direction transverse—
30Comparative tracking index (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)standard IEC 60112test liquid A—
31Melt volume rate (Akro)Typical value printed on the manufacturer product pagegrade PRECITE P3 GF 30 natural (6850)standard ISO 1133temperature 250 °Cload 2.16 kg—
32Equilibrium water uptake at 35 °C (Borges et al.)Measured in water immersion and printed in Table 2 of the papermaterial PBT-GF30 as tested in Borges et al. (grade not named)test water immersion, equilibrium M-infinitytemperature 35 °C—
33Equilibrium water uptake at 70 °C (Borges et al.)Measured in water immersion and printed in Table 2 of the papermaterial PBT-GF30 as tested in Borges et al. (grade not named)test water immersion, equilibrium M-infinitytemperature 70 °C—
34Equilibrium water uptake at 130 °C (Borges et al.)Measured in water immersion and printed in Table 2 of the papermaterial PBT-GF30 as tested in Borges et al. (grade not named)test water immersion, equilibrium M-infinitytemperature 130 °C—
35Young's modulus, room temperature, standard specimens (Borges et al.)Bulk tensile test printed in the mechanical properties text, tensile rate 1 mm/minmaterial PBT-GF30 as tested in Borges et al. (grade not named)condition dry as suppliedtemperature room temperaturespecimen standardUncertainty: ± 0.1 GPa (printed)
36Tensile strength, room temperature, standard specimens (Borges et al.)Bulk tensile test printed in the mechanical properties text, tensile rate 1 mm/minmaterial PBT-GF30 as tested in Borges et al. (grade not named)condition dry as suppliedtemperature room temperaturespecimen standardUncertainty: ± 1 MPa (printed)
37Young's modulus at 70 °C (Borges et al.)Bulk tensile test printed in the mechanical properties tablematerial PBT-GF30 as tested in Borges et al. (grade not named)condition dry as supplied, tested at temperaturetemperature 70 °CUncertainty: ± 0.1 GPa (printed)
38Tensile strength at 70 °C (Borges et al.)Bulk tensile test printed in the mechanical properties tablematerial PBT-GF30 as tested in Borges et al. (grade not named)condition dry as supplied, tested at temperaturetemperature 70 °CUncertainty: ± 1 MPa (printed)
39Young's modulus at 130 °C (Borges et al.)Bulk tensile test printed in the mechanical properties tablematerial PBT-GF30 as tested in Borges et al. (grade not named)condition dry as supplied, tested at temperaturetemperature 130 °CUncertainty: ± 0.1 GPa (printed)
40Tensile strength at 130 °C (Borges et al.)Bulk tensile test printed in the mechanical properties tablematerial PBT-GF30 as tested in Borges et al. (grade not named)condition dry as supplied, tested at temperaturetemperature 130 °CUncertainty: ± 1 MPa (printed)
41Glass transition temperature (Borges et al.)Value printed in the Borges et al. 2021 test conditions sectionmaterial PBT-GF30 as tested in Borges et al. (grade not named)Uncertainty: ± 4 °C (printed)
42Density, safety information range (tbgroup)Range printed in the supplier safety information (not a datasheet value)grade PBT GF30, supplier safety informationunit as printed g/ccm—
43Melting point, safety information range (tbgroup)Range printed in the supplier safety information (not a datasheet value)grade PBT GF30, supplier safety information—
44Flash point (tbgroup)Value printed in the supplier safety information as a lower boundgrade PBT GF30, supplier safety informationprinted as > 400 °C—
45Ignition point (tbgroup)Value printed in the supplier safety information as a lower boundgrade PBT GF30, supplier safety informationprinted as > 350 °C—
46Thermal decomposition onset (tbgroup)Value printed in the supplier safety information as a lower boundgrade PBT GF30, supplier safety informationprinted as > 290 °C—

Corrosion and compatibility

What happens when it meets other materials and environments.

Corrosion and compatibility
EnvironmentConcernWhat happens
Hot water above 60 °C moderate PBT is sensitive to hot water above 60 °C, according to Wikipedia.1
Water immersion at 35 °C, 70 °C and 130 °C moderate Equilibrium water uptake rises from 0.47 % at 35 °C to 0.56 % at 130 °C in PBT-GF30 tested by Borges et al.2
Heat and water together above 80 °C moderate Borges et al. report a chemical change in the OH profile between 80 and 85 °C.3
Changing climate with low moisture absorption low Akro states that the grade has low moisture absorption, giving consistent properties in changing climates.4
Corrosion details
#EnvironmentDetailsTest conditions
1 Hot water above 60 °C Wikipedia states that PBT and PET are sensitive to hot water above 60 °C (140 °F). The page does not use the word hydrolysis, and it gives no test condition or glass-fibre content for this statement. basis general statement for PBT, not tested on this grade
2 Water immersion at 35 °C, 70 °C and 130 °C Borges et al. 2021 state that the water diffusion behaviour is Fickian, and print equilibrium uptake M-infinity values of 0.47 %, 0.50 % and 0.56 % at 35, 70 and 130 °C. The paper says tensile values after water ageing appear only in a figure. material PBT-GF30 as tested in Borges et al. (grade not named)test water immersion
3 Heat and water together above 80 °C Borges et al. report that the OH⁻ profile change in FTIR occurs between 80 and 85 °C, which the paper treats as the point where the chemical change becomes visible. The paper prints no mass loss figure for this effect. material PBT-GF30 as tested in Borges et al. (grade not named)test FTIR after water exposure
4 Changing climate with low moisture absorption Akro states that low moisture absorption gives consistent mechanical and electrical properties under changing climatic conditions. The page gives the 0.2 % and 0.4 % absorption values recorded in the properties table, and no ageing test. basis manufacturer statement with absorption values from the property table

Risks and side effects

Hazards to people, what happens when a cell overheats, and how the material is handled and stored.

For people

The one safety information sheet read classifies this grade as not hazardous under the cited EC rules.

Classification
The tbgroup safety information prints Potential hazards: None and states that the product is not classified by the Dangerous Chemicals Ordinance or EC guidelines.
Dust
Dust from grinding may form an explosible dust-air mixture if dispersed, so dust is removed by suction.

If it fails

The failure routes in these sources are heat and water, and the heat route releases toxic gases.

Heat
Above 290 °C the product may release toxic gases, including traces of hydrogen cyanide, according to the safety information.
Water
Borges et al. measured an equilibrium water uptake of 0.56 % at 130 °C, and tensile strength of 44 MPa at 130 °C on dry specimens.

Test details
The original wording and numbers from the sources, for readers who want them.

Failure risks

Failure risks
FailureTrigger and consequence
Thermal decomposition at high temperaturehigh severityHeating above 290 °C during processing or in a fireToxic gases, including traces of hydrogen cyanide, carbon monoxide, tetrahydrofuran and terephthalic acid, are possibly released above 290 °C (tbgroup safety information).
Loss of stiffness and strength at elevated temperaturemoderate severityUse above room temperature (Borges et al. tested dry specimens at the test temperature)Young's modulus falls to 4.6 GPa at 70 °C and 2.3 GPa at 130 °C, and tensile strength falls to 66 MPa at 70 °C and 44 MPa at 130 °C, against 8.6 GPa and 112 MPa at room temperature (dry as supplied).

Handling and storage

  • Provide adequate ventilation and local exhaust as needed, and withdraw dust by suction, according to the safety information.
  • Take precautionary measures against static discharges and keep away from sources of ignition during processing.

Supply and geography

How common the raw materials are and where they come from.

Terephthalic acid (monomer)

Wikipedia states that several million tons are produced annually, with no year or tonnage printed.

1,4-Butanediol (monomer)

Wikipedia states that about one million metric tons per year are produced worldwide, with no year printed for that figure.

Glass fibre (reinforcement)

Wikipedia gives no production figure for glass fibre. It describes E-glass as an alumino-borosilicate glass with less than 1% w/w alkali oxides, mainly used for glass-reinforced plastics.

Updated