Nichrome NiCr 80/20
Nickel-chromium alloy, about 80 % Ni and 20 % Cr by mass
Also known as UNS N06003, EN 2.4869, EN name NiCr 80-20, DIN 17470, ASTM B344, Nichrome
Nichrome is the nickel-chromium resistance alloy with about 80 % nickel and 20 % chromium, sold as NiCr 80/20 (UNS N06003, material 2.4869).
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Carry current as a heater
1.09 Ohm mm2/m
Stay solid when hot
1400 °C melting point
Stay light
8.30 g/cm3
Strength in fine wire
810 MPa tensile
Recipe, share of the weight
- Ni 80%Nickel
- Cr 20%Chromium
Best for
Carrying current as a heater: 1.09 Ohm mm2/m resistivity with a continuous limit of 1200 °C in air, and a chromium oxide scale that resists oxidation
Weakest at
Strength at temperature: 15 MPa for 1 % creep in 1000 h at 800 °C and 4 MPa at 1000 °C, and a thermal conductivity of only 15 W/(m·K)
Risk at a glance
- People Low. Mixed classification
- If it fails Moderate. Oxidation above the service limit
- Corrosion Low. A chromium oxide scale protects the alloy from oxidation up to about 1150 °C.
Quick facts: NiCr 80/20
| Property | Value | Basis |
|---|---|---|
| Density | 8.3 to 8.4 g/cm³ | 2 sourced values across conditions |
| Yield strength | 300 to 420 MPa | 2 sourced values across conditions |
| Tensile strength | 725 to 810 MPa | 2 sourced values across conditions |
| Thermal conductivity | 15 W/(m·K) | 1 sourced value |
| Thermal expansion (CTE) | 14.1 to 17.2 ppm/K | 2 sourced values across conditions |
| Melting point | 1,400 °C | 1 sourced value |
| Specific heat | 460 J/(kg·K) | 1 sourced value |
| Electrical resistivity | 0.0000011 Ω·m | 2 sourced values across conditions |
| Maximum service temperature | 1,150 to 1,200 °C | 2 sourced values across conditions |
What is the density of Nichrome (NiCr 80/20)?
Nichrome (NiCr 80/20) has a density of 8.3 to 8.4 g/cm³. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the thermal conductivity of Nichrome (NiCr 80/20)?
Nichrome (NiCr 80/20) has a thermal conductivity of 15 W/(m·K). The source and test conditions are listed in the properties table on this page.
What is the coefficient of thermal expansion of Nichrome (NiCr 80/20)?
Nichrome (NiCr 80/20) has a coefficient of thermal expansion of 14.1 to 17.2 ppm/K. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the melting point of Nichrome (NiCr 80/20)?
Nichrome (NiCr 80/20) has a melting point of 1,400 °C. The source and test conditions are listed in the properties table on this page.
What is the yield strength of Nichrome (NiCr 80/20)?
Nichrome (NiCr 80/20) has a yield strength of 300 to 420 MPa. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What are the other names and codes for Nichrome (NiCr 80/20)?
Nichrome (NiCr 80/20) is also written as UNS N06003, EN 2.4869, EN name NiCr 80-20, DIN 17470, ASTM B344, Nichrome. Each code is printed in the source listed beside it in the designations table.
What is Nichrome (NiCr 80/20) used for?
Uses recorded in the sources include Resistance heating elements; Precision wire-wound resistors; Burn-wire release actuator for a CubeSat tie-down.
Why it exists
Nichrome is a heating alloy. It combines high electrical resistance with a protective chromium oxide scale, so it can carry current and turn it into heat in air at high temperature. Kanthal's Nikrothal 80 wire has a resistivity of 1.09 Ohm mm2/m at 20 °C, a melting point of 1400 °C and a continuous limit of 1200 °C in air. It is found in heating elements, in precision resistors, and in burn-wire release mechanisms on CubeSats. Its weak points are its low thermal conductivity, 15 W/(m·K) at 20 °C, and its loss of strength at temperature.
Where it's used
Heating elements
Heating elements are the main use. Goodfellow lists electric furnaces, kilns, toasters, hair dryers and industrial heating equipment, and Wikipedia adds kettles, heat guns and space heaters.
Burn-wire releases in CubeSats
A JPL tie-down and release mechanism uses 30 AWG nichrome wire to cut a Vectran cable. The source gives a current of 1.6 A applied for about 5 to 10 seconds.
Solar panel deployment
Wikipedia says nichrome is used in the solar panel deployment mechanism of spacecraft, citing LightSail-A.
Recipe
Nickel-chromium alloy, about 80 % Ni and 20 % Cr by mass; Kanthal Nikrothal 80 composition: Ni balance, Cr 19.0 to 21.0 %, Si 1.0 to 1.7 %, Mn up to 1.0 %, C up to 0.10 %
Nichrome is a two-element alloy of nickel and chromium, about 80 % nickel and 20 % chromium by mass (Wikipedia, Goodfellow and Studer SA). Kanthal's datasheet gives the chromium range as 19.0 to 21.0 %, with nickel as the balance.
| Ingredient | Share of the weight | What it does |
|---|---|---|
| Nickel Ni | 80% | The matrix of the alloy. The balance of the Kanthal composition is nickel. |
| Chromium Cr | 20% | Forms the protective chromium oxide (Cr2O3) scale that resists oxidation in air (Goodfellow). |
Weight shares are as printed in the sources.
What it can do
Carry current as a heater
1.09 Ohm mm2/m
measured
The electrical resistivity of Nikrothal 80 is 1.09 Ohm mm2/m at 20 °C, and the Goodfellow range is 1.08 to 1.12 µΩ·m at room temperature.
Stay solid when hot
1400 °C melting point
measured
The melting point is 1400 °C. The continuous operating limit in air is 1200 °C.
Stay light
8.30 g/cm3
measured
Density is 8.30 g/cm3 in the Kanthal datasheet, and about 8.4 g/cm3 in the Goodfellow page.
Strength in fine wire
810 MPa tensile
measured
In 1.0 mm wire the datasheet gives 810 MPa tensile strength, 420 MPa yield and 30 % elongation at room temperature.
How it compares
This profile has no second heating alloy read in the same run, so the compare rows use nichrome's own figures: resistivity, continuous temperature limit and thermal conductivity. Read them as nichrome's values, not as a ranking against another metal.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Other materials are shown beside it; each was measured under its own conditions, so open its page before comparing closely. Compare every grade in the family.
| Measurement | NiCr 80/20 | KN | Ni-10Cr (Chromel-P) | Ni-Cr-Al-Cu precision resistance alloy |
|---|---|---|---|---|
| Thermal behavior and safety | ||||
| Melting point, Nikrothal 80Value printed in a manufacturer datasheet | 1400 °C | 1399 °C | 1430 °C | 1350 °C |
| Thermal conductivity at 20 °C, Nikrothal 80Value printed in a manufacturer datasheet | 15 W/(m·K)7 | 0.297 W/(cm·°C) | 19.2 W/(m·K) | 14.6 W/(m·K) |
| Specific heat capacity at 20 °C, Nikrothal 80Value printed in a manufacturer datasheet | 0.46 kJ/(kg·K)8 | 0.523 J/(g·K) | 0.448 kJ/(kg·K) | 435 J/(kg·K) |
| Physical and electrical | ||||
| Density, Nikrothal 80 wireValue printed in a manufacturer datasheet | 8.3 g/cm³1 | 8.6 g/cm³ | 8.72 g/cm³ | 8.1 g/cm³ |
| Density, Ni80/Cr20 wire (approximate) | 8.4 g/cm³2 | 8.6 g/cm³ | 8.72 g/cm³ | 8.1 g/cm³ |
| Electrical resistivity at 20 °C, Nikrothal 80Value printed in a manufacturer datasheet | 1.09 Ω mm2/m3 | 29.4 µΩ·cm | 0.706 Ω mm2/m | 133 µΩ·cm |
| Electrical resistivity, Ni80/Cr20 at room temperature | 1.08 to 1.12 µΩ·m4 | 29.4 µΩ·cm | 0.706 Ω mm2/m | 133 µΩ·cm |
| Hardness Hv, 1.0 mm wire, room temperatureValue printed in a manufacturer datasheet | 180 HV17 | no data | 140 HV | 160 to 280 HV |
| Other measurements | ||||
| Maximum continuous operating temperature in air, Nikrothal 80Value printed in a manufacturer datasheet | 1200 °C5 | no data | 900 °C | 300 °C |
| Oxidation resistance limit, Ni80/Cr20 wire | 1150 °C6 | no data | 900 °C | 300 °C |
| Coefficient of thermal expansion, 20 to 250 °C, Nikrothal 80Value printed in a manufacturer datasheet | 14.1 ppm/K9 | 12 ppm/K | 17 ppm/K | 13 ppm/K |
| Coefficient of thermal expansion, 20 to 1000 °C, Nikrothal 80Value printed in a manufacturer datasheet | 17.2 ppm/K10 | 12 ppm/K | 17 ppm/K | 13 ppm/K |
| Yield strength Rp0.2, 1.0 mm wire, room temperatureValue printed in a manufacturer datasheet | 420 MPa11 | 40 ksi | 45 ksi | > 300 MPa |
| Yield strength Rp0.2, 4.0 mm wire, room temperatureValue printed in a manufacturer datasheet | 300 MPa12 | 40 ksi | 45 ksi | > 300 MPa |
| Tensile strength Rm, 1.0 mm wire, room temperatureValue printed in a manufacturer datasheet | 810 MPa13 | 85 ksi | 95 ksi | 650 to 900 MPa |
| Tensile strength Rm, 4.0 mm wire, room temperatureValue printed in a manufacturer datasheet | 725 MPa14 | 85 ksi | 95 ksi | 650 to 900 MPa |
| Ultimate tensile strength at 900 °C, Nikrothal 80Value printed in a manufacturer datasheet | 100 MPa15 | 85 ksi | 95 ksi | 650 to 900 MPa |
| Elongation A, 1.0 mm wire, room temperatureValue printed in a manufacturer datasheet | 30 %16 | 35 % | 35 % | > 30 % |
| Creep strength for 1 % elongation in 1000 h at 800 °C, Nikrothal 80Value printed in a manufacturer datasheet | 15 MPa18 | no data | no data | no data |
| Creep strength for 1 % elongation in 1000 h at 1000 °C, Nikrothal 80Value printed in a manufacturer datasheet | 4 MPa19 | no data | no data | no data |
| Emissivity, fully oxidized materialValue printed in a manufacturer datasheet | 0.88 -20 | no data | no data | no data |
Why choose it, and why not
Good for
- Heating elements: 1.09 Ohm mm2/m resistivity and a continuous limit of 1200 °C in air (Kanthal).
- Oxidation resistance: a chromium oxide scale resists oxidation up to about 1150 °C (Goodfellow).
- Fine wire at room temperature: 810 MPa tensile strength and 30 % elongation for 1.0 mm wire (Kanthal).
Watch out for
- Creep: 15 MPa for 1 % elongation in 1000 h at 800 °C, and 4 MPa at 1000 °C.
- Low thermal conductivity: 15 W/(m·K) at 20 °C.
- Hazard classification varies by supplier: Airgas classifies its nickel wire as Not Classified.
- No corrosion rate, outgassing or radiation data were found.
Nichrome 80/20 is the standard heating alloy, with a resistivity of 1.09 Ohm mm2/m, a 1400 °C melting point and a 1200 °C continuous limit in air. It is a good choice for a heater, but its strength falls sharply at 800 °C and above, and the profile has no corrosion-rate, outgassing or radiation values.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Other names and standards
The same grade under other systems, as datasheets and standards print them. Each code was checked against the page it comes from.
| System | Codes |
|---|---|
| UNS | N06003 |
| EN | 2.4869 |
| EN name | NiCr 80-20 |
| DIN | 17470 (DIN 17470:1984-10, heating conductor alloys) |
| ASTM | B344 |
| Trade name | Nichrome (family name used for the 80/20 grade) |
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Density, Nikrothal 80 wire | — | grade Nikrothal 80 (Kanthal)temperature not statedform wire; the datasheet does not state a diameter for the physical values | — |
| 2 | Density, Ni80/Cr20 wire (approximate) | Approximate value printed on a supplier material information page | grade Ni80/Cr20temperature not stated | Goodfellow prints approximately 8.4 g/cm3, about 1 % above the 8.30 g/cm3 that Kanthal prints for Nikrothal 80. Both are kept; the Kanthal value is the datasheet figure. |
| 3 | Electrical resistivity at 20 °C, Nikrothal 80 | — | grade Nikrothal 80 (Kanthal)temperature 20 °Cform wire; the datasheet does not state a diameter for this value | — |
| 4 | Electrical resistivity, Ni80/Cr20 at room temperature | Range printed on a supplier material information page | grade Ni80/Cr20temperature room temperature (not stated more precisely) | Wikipedia prints about 1.12 µΩ·m for the 80/20 alloy and a family range of 1.0 to 1.5 µΩ·m. Kanthal's 1.09 Ohm mm2/m (1.09 µΩ·m) sits inside the Goodfellow range. |
| 5 | Maximum continuous operating temperature in air, Nikrothal 80 | — | grade Nikrothal 80 (Kanthal)environment air, continuous operationform wire | — |
| 6 | Oxidation resistance limit, Ni80/Cr20 wire | Limit printed on a supplier material information page | grade Ni80/Cr20environment air, high-temperature oxidation | The same Goodfellow page gives continuous-duty applications up to 1100 °C, below the 1150 °C oxidation limit, and Kanthal sets 1200 °C as the continuous limit. The three limits are not the same test. |
| 7 | Thermal conductivity at 20 °C, Nikrothal 80 | — | grade Nikrothal 80 (Kanthal)temperature 20 °Cunit in source W m-1 K-1 | — |
| 8 | Specific heat capacity at 20 °C, Nikrothal 80 | — | grade Nikrothal 80 (Kanthal)temperature 20 °Cunit in source kJ kg-1 K-1 | — |
| 9 | Coefficient of thermal expansion, 20 to 250 °C, Nikrothal 80 | — | grade Nikrothal 80 (Kanthal)temperature 20 to 250 °Cunit in source x10-6/K | — |
| 10 | Coefficient of thermal expansion, 20 to 1000 °C, Nikrothal 80 | — | grade Nikrothal 80 (Kanthal)temperature 20 to 1000 °Cunit in source x10-6/K | — |
| 11 | Yield strength Rp0.2, 1.0 mm wire, room temperature | — | grade Nikrothal 80 (Kanthal)form wire, diameter 1.0 mmtemperature room temperaturetemper not stated | — |
| 12 | Yield strength Rp0.2, 4.0 mm wire, room temperature | — | grade Nikrothal 80 (Kanthal)form wire, diameter 4.0 mmtemperature room temperaturetemper not stated | — |
| 13 | Tensile strength Rm, 1.0 mm wire, room temperature | — | grade Nikrothal 80 (Kanthal)form wire, diameter 1.0 mmtemperature room temperaturetemper not stated | — |
| 14 | Tensile strength Rm, 4.0 mm wire, room temperature | — | grade Nikrothal 80 (Kanthal)form wire, diameter 4.0 mmtemperature room temperaturetemper not stated | — |
| 15 | Ultimate tensile strength at 900 °C, Nikrothal 80 | — | grade Nikrothal 80 (Kanthal)temperature 900 °Cdeformation rate 6.2 x 10-2/minform not stated | — |
| 16 | Elongation A, 1.0 mm wire, room temperature | — | grade Nikrothal 80 (Kanthal)form wire, diameter 1.0 mmtemperature room temperaturetemper not stated | — |
| 17 | Hardness Hv, 1.0 mm wire, room temperature | — | grade Nikrothal 80 (Kanthal)form wire, diameter 1.0 mmtemperature room temperature | Non-canonical property name; hardness_vickers is not in the canonical property file. |
| 18 | Creep strength for 1 % elongation in 1000 h at 800 °C, Nikrothal 80 | — | grade Nikrothal 80 (Kanthal)temperature 800 °Ctime 1000 hcriterion 1 % elongation | Non-canonical property name; the datasheet gives it under the elevated temperature mechanical properties section. |
| 19 | Creep strength for 1 % elongation in 1000 h at 1000 °C, Nikrothal 80 | — | grade Nikrothal 80 (Kanthal)temperature 1000 °Ctime 1000 hcriterion 1 % elongation | Non-canonical property name. |
| 20 | Emissivity, fully oxidized material | — | grade Nikrothal 80 (Kanthal)surface fully oxidized | Non-canonical property name. The datasheet gives this for fully oxidized material only. |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Air at high temperature | low | A chromium oxide scale protects the alloy from oxidation up to about 1150 °C.1 |
| Air, continuous operation at elevated temperature | low | Kanthal rates the wire for continuous use in air up to 1200 °C.2 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Air at high temperature | Goodfellow attributes the high-temperature oxidation resistance to a protective chromium oxide (Cr2O3) scale and gives the limit as up to 1150 °C. The page gives no oxidation rate or weight gain. | environment airbasis supplier material information page; no test duration stated |
| 2 | Air, continuous operation at elevated temperature | The datasheet gives 1200 °C as the maximum continuous operating temperature in air and describes the alloy as having good oxidation resistance and very good form stability. No mass loss or scale thickness is given. | environment airform wire |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
The alloy is about 80 % nickel and 20 % chromium. The sources do not agree on its hazard classification, so the raw materials are the better guide.
- Supplier classification
- The Airgas nickel wire and rod sheet is classified as Not Classified under GHS and has no signal word. Other suppliers' listings of 80/20 nickel-chromium wire, seen only in search snippets, carry H317 and H351.
- Proposition 65
- The same Airgas sheet lists nickel and hexavalent chromium compounds as carcinogens under California Proposition 65.
If it fails
The failure routes in the sources are temperature and load. The datasheet gives limits but no failure rates.
- Overheating
- Kanthal gives 1200 °C as the continuous limit in air. Goodfellow gives an oxidation limit of 1150 °C. Neither source gives a time to failure above these limits.
- Creep
- At 800 °C the datasheet gives 15 MPa for 1 % elongation in 1000 h, and at 1000 °C it gives 4 MPa.
Handling and storage
- Keep it below the limit
- Kanthal gives 1200 °C as the maximum continuous operating temperature in air. Keep loaded wires below that and well below it when they carry tension.
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Oxidation above the service limitmoderate severity | Operation above 1200 °C continuous in air (Kanthal), or above the 1150 °C oxidation limit (Goodfellow)Both sources give a temperature limit. Neither gives an oxidation rate, so the time to failure above the limit cannot be taken from these sources. |
| Creep sag under sustained load at high temperaturemoderate severity | A sustained stress at 800 °C or above, for example a wire carrying a tension load in a furnaceThe datasheet gives 15 MPa for 1 % elongation in 1000 h at 800 °C and 4 MPa at 1000 °C, so the allowable sustained stress falls sharply with temperature. |
Side effects on surrounding parts
| Affects | Effect |
|---|---|
| Handling of dust and fume from grinding or welding | Nickel and chromium make up nearly all of the alloy, so the sources classify its raw materials, not the finished wire, as the hazard. Airgas lists nickel and hexavalent chromium compounds on Proposition 65. |
Handling and storage
- The datasheet gives a maximum continuous operating temperature of 1200 °C in air. Use a lower limit for loaded wires, since creep strength at 800 °C is only 15 MPa for 1 % elongation in 1000 h.
Supply and geography
How common the raw materials are and where they come from.
Nickel
- Top producers (2025)
- Indonesia 66.7%, Philippines 6.9%, Russia 5.1%, Canada 3.6%
- Recycling
- USGS: nickel recovered from scrap accounted for approximately 60 % of apparent consumption in 2025. Most secondary nickel is stainless-steel scrap.
- Substitutes
- USGS: low-nickel, duplex or ultrahigh-chromium stainless steels replace austenitic grades in some uses; titanium alloys can substitute for nickel or nickel-base alloys in corrosive environments.
Chromium
- Top producers (2025)
- South Africa 45.1%, Turkey 17.6%, Kazakhstan 13.7%
- Recycling
- USGS: recycled chromium in reported stainless-steel scrap receipts accounted for 21 % of supply in 2025.
- Substitutes
- USGS: chromium has no substitute in stainless steel or in superalloys.
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: nichrome
spore_version: 0.2
family: resistance-and-thermocouple-alloys
name: Nichrome
abbreviation: NiCr 80/20
role: resistance heating alloy
category: metals
type: nickel-superalloys
summary: |
Nichrome is the nickel-chromium resistance alloy with about 80 % nickel and 20 % chromium, sold as NiCr 80/20 (UNS N06003, material 2.4869). Its electrical resistivity is 1.09 Ohm mm2/m at 20 °C, its melting point is about 1400 °C, and Kanthal gives a maximum continuous operating temperature in air of 1200 °C. It is soft and ductile at room temperature in fine wire (810 MPa tensile strength and 30 % elongation for 1.0 mm wire), but its strength falls quickly with temperature: 15 MPa gives 1 % creep in 1000 h at 800 °C.
best_for: 'Carrying current as a heater: 1.09 Ohm mm2/m resistivity with a continuous limit of 1200 °C in air, and a chromium oxide scale that resists oxidation'
weakest_at: 'Strength at temperature: 15 MPa for 1 % creep in 1000 h at 800 °C and 4 MPa at 1000 °C, and a thermal conductivity of only 15 W/(m·K)'
identity:
formula: 'Nickel-chromium alloy, about 80 % Ni and 20 % Cr by mass; Kanthal Nikrothal 80 composition: Ni balance, Cr 19.0 to 21.0 %, Si 1.0 to 1.7 %, Mn up to 1.0 %, C up to 0.10 %'
source: kanthal-nikrothal80
where: Chemical composition table of the Kanthal Nikrothal 80 wire datasheet (Ni Bal., Cr 19.0 to 21.0, Si 1.0 to 1.7, Mn 1.0 max, C 0.10 max). The composition of the 80/20 grade is also given as 80 % nickel and 20 % chromium in the Goodfellow and Wikipedia pages.
designations:
- system: UNS
code: N06003
source: studersa-24869
where: Page title and Description section, '2.4869 - Resistance alloy / NiCr 80-20 / N06003'
- system: EN
code: '2.4869'
source: studersa-24869
where: Page title and Description section, 'Material 2.4869'
- system: EN name
code: NiCr 80-20
source: studersa-24869
where: Page title and Description section, 'also known as NiCr 80-20'
- system: ASTM
code: B344
source: bobmartin-8020
where: Specification line of the 80/20 Nichrome Wire product page, printed as ASTM-B-344
- system: DIN
code: '17470'
note: DIN 17470:1984-10, heating conductor alloys
source: wikipedia-nichrome
where: Designations section, DIN 17470:1984-10
- system: Trade name
code: Nichrome
note: family name used for the 80/20 grade
source: wikipedia-nichrome
where: Page title; the article describes nichrome as a family of nickel-chromium alloys
tags:
environments: []
stresses:
- extreme-heat
applications:
- thermal-control
- electronics-and-chips
- mechanisms
properties:
- benchmark: density
label: Density, Nikrothal 80 wire
value: 8.3
unit: g/cm3
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
temperature: not stated
form: wire; the datasheet does not state a diameter for the physical values
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Physical properties section, Density
- benchmark: density
label: Density, Ni80/Cr20 wire (approximate)
value: 8.4
unit: g/cm3
scope: material
conditions:
grade: Ni80/Cr20
temperature: not stated
method: Approximate value printed on a supplier material information page
status: ground
note: Goodfellow prints approximately 8.4 g/cm3, about 1 % above the 8.30 g/cm3 that Kanthal prints for Nikrothal 80. Both are kept; the Kanthal value is the datasheet figure.
source: goodfellow-nicr80
where: Material Overview section, density sentence
- benchmark: melting_point
label: Melting point, Nikrothal 80
value: 1400
unit: °C
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
pressure: not stated
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Physical properties section, Melting point
- benchmark: electrical_resistivity
label: Electrical resistivity at 20 °C, Nikrothal 80
value: 1.09
unit: Ω mm2/m
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
temperature: 20 °C
form: wire; the datasheet does not state a diameter for this value
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Physical properties section, Electrical resistivity at 20°C
- benchmark: electrical_resistivity
label: Electrical resistivity, Ni80/Cr20 at room temperature
value: 1.08
value_high: 1.12
bound: range
unit: µΩ·m
scope: material
conditions:
grade: Ni80/Cr20
temperature: room temperature (not stated more precisely)
method: Range printed on a supplier material information page
status: ground
note: Wikipedia prints about 1.12 µΩ·m for the 80/20 alloy and a family range of 1.0 to 1.5 µΩ·m. Kanthal's 1.09 Ohm mm2/m (1.09 µΩ·m) sits inside the Goodfellow range.
source: goodfellow-nicr80
where: Material Overview section, electrical resistivity sentence
- benchmark: max_service_temp
label: Maximum continuous operating temperature in air, Nikrothal 80
value: 1200
unit: °C
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
environment: air, continuous operation
form: wire
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Physical properties section, Max continuous operating temperature in air
- benchmark: max_service_temp
label: Oxidation resistance limit, Ni80/Cr20 wire
value: 1150
unit: °C
scope: material
conditions:
grade: Ni80/Cr20
environment: air, high-temperature oxidation
method: Limit printed on a supplier material information page
status: ground
note: The same Goodfellow page gives continuous-duty applications up to 1100 °C, below the 1150 °C oxidation limit, and Kanthal sets 1200 °C as the continuous limit. The three limits are not the same test.
source: goodfellow-nicr80
where: Material Overview section, oxidation resistance sentence
- benchmark: thermal_conductivity
label: Thermal conductivity at 20 °C, Nikrothal 80
value: 15
unit: W/(m·K)
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
temperature: 20 °C
unit_in_source: W m-1 K-1
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Thermal conductivity table, column Temp 20 °C
- benchmark: specific_heat
label: Specific heat capacity at 20 °C, Nikrothal 80
value: 0.46
unit: kJ/(kg·K)
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
temperature: 20 °C
unit_in_source: kJ kg-1 K-1
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Specific heat capacity table, column Temp 20
- benchmark: cte
label: Coefficient of thermal expansion, 20 to 250 °C, Nikrothal 80
value: 14.1
unit: ppm/K
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
temperature: 20 to 250 °C
unit_in_source: x10-6/K
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Coefficient of thermal expansion section, row 20 to 250 °C
- benchmark: cte
label: Coefficient of thermal expansion, 20 to 1000 °C, Nikrothal 80
value: 17.2
unit: ppm/K
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
temperature: 20 to 1000 °C
unit_in_source: x10-6/K
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Coefficient of thermal expansion section, row 20 to 1000 °C
- benchmark: yield_strength
label: Yield strength Rp0.2, 1.0 mm wire, room temperature
value: 420
unit: MPa
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
form: wire, diameter 1.0 mm
temperature: room temperature
temper: not stated
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Mechanical properties, room temperature table, row 1.0 mm, column Yield Rp0.2
- benchmark: yield_strength
label: Yield strength Rp0.2, 4.0 mm wire, room temperature
value: 300
unit: MPa
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
form: wire, diameter 4.0 mm
temperature: room temperature
temper: not stated
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Mechanical properties, room temperature table, row 4.0 mm, column Yield Rp0.2
- benchmark: ultimate_tensile_strength
label: Tensile strength Rm, 1.0 mm wire, room temperature
value: 810
unit: MPa
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
form: wire, diameter 1.0 mm
temperature: room temperature
temper: not stated
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Mechanical properties, room temperature table, row 1.0 mm, column Tensile Rm
- benchmark: ultimate_tensile_strength
label: Tensile strength Rm, 4.0 mm wire, room temperature
value: 725
unit: MPa
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
form: wire, diameter 4.0 mm
temperature: room temperature
temper: not stated
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Mechanical properties, room temperature table, row 4.0 mm, column Tensile Rm
- benchmark: ultimate_tensile_strength
label: Ultimate tensile strength at 900 °C, Nikrothal 80
value: 100
unit: MPa
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
temperature: 900 °C
deformation_rate: 6.2 x 10-2/min
form: not stated
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Mechanical properties at elevated temperature section, Ultimate tensile strength at 900 °C
- benchmark: elongation
label: Elongation A, 1.0 mm wire, room temperature
value: 30
unit: '%'
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
form: wire, diameter 1.0 mm
temperature: room temperature
temper: not stated
method: Value printed in a manufacturer datasheet
status: ground
source: kanthal-nikrothal80
where: Mechanical properties, room temperature table, row 1.0 mm, column Elongation A
- benchmark: hardness_vickers
label: Hardness Hv, 1.0 mm wire, room temperature
value: 180
unit: HV
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
form: wire, diameter 1.0 mm
temperature: room temperature
method: Value printed in a manufacturer datasheet
status: ground
note: Non-canonical property name; hardness_vickers is not in the canonical property file.
source: kanthal-nikrothal80
where: Mechanical properties, room temperature table, row 1.0 mm, column Hardness (Hv)
- benchmark: creep_strength_1pct_1000h
label: Creep strength for 1 % elongation in 1000 h at 800 °C, Nikrothal 80
value: 15
unit: MPa
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
temperature: 800 °C
time: 1000 h
criterion: 1 % elongation
method: Value printed in a manufacturer datasheet
status: ground
note: Non-canonical property name; the datasheet gives it under the elevated temperature mechanical properties section.
source: kanthal-nikrothal80
where: Mechanical properties at elevated temperature section, Creep strength, 1 % elongation in 1000 h, 800 °C
- benchmark: creep_strength_1pct_1000h
label: Creep strength for 1 % elongation in 1000 h at 1000 °C, Nikrothal 80
value: 4
unit: MPa
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
temperature: 1000 °C
time: 1000 h
criterion: 1 % elongation
method: Value printed in a manufacturer datasheet
status: ground
note: Non-canonical property name.
source: kanthal-nikrothal80
where: Mechanical properties at elevated temperature section, Creep strength, 1 % elongation in 1000 h, 1000 °C
- benchmark: emissivity
label: Emissivity, fully oxidized material
value: 0.88
unit: '-'
scope: material
conditions:
grade: Nikrothal 80 (Kanthal)
surface: fully oxidized
method: Value printed in a manufacturer datasheet
status: ground
note: Non-canonical property name. The datasheet gives this for fully oxidized material only.
source: kanthal-nikrothal80
where: Physical properties section, Emissivity
corrosion:
- environment: Air at high temperature
headline: A chromium oxide scale protects the alloy from oxidation up to about 1150 °C.
effect: Goodfellow attributes the high-temperature oxidation resistance to a protective chromium oxide (Cr2O3) scale and gives the limit as up to 1150 °C. The page gives no oxidation rate or weight gain.
rating: low
conditions:
environment: air
basis: supplier material information page; no test duration stated
source: goodfellow-nicr80
where: Material Overview section, oxidation resistance sentence
- environment: Air, continuous operation at elevated temperature
headline: Kanthal rates the wire for continuous use in air up to 1200 °C.
effect: The datasheet gives 1200 °C as the maximum continuous operating temperature in air and describes the alloy as having good oxidation resistance and very good form stability. No mass loss or scale thickness is given.
rating: low
conditions:
environment: air
form: wire
source: kanthal-nikrothal80
where: Physical properties section, Max continuous operating temperature in air; description paragraph
risks:
hazards:
- text: 'Airgas nickel wire and rod safety data sheet (approval 2-1-2016): GHS Hazard Classification is ''Not Classified'' and the label has no symbol or signal word. This sheet covers a nickel wire and rod product whose list includes 80/20 nickel-chromium; the sheet does not name Ni80/Cr20 as a product of its own.'
ghs: []
source: airgas-nickel-sds
where: Section 2, GHS Hazard Classification line; header block with approval date
- text: The same Airgas sheet lists nickel (listed 10-1-1989) and hexavalent chromium compounds (listed 2-27-1987) under California Proposition 65 carcinogens.
ghs: []
source: airgas-nickel-sds
where: Regulatory information section, California Proposition 65 line
failure_risks:
- mode: Oxidation above the service limit
trigger: Operation above 1200 °C continuous in air (Kanthal), or above the 1150 °C oxidation limit (Goodfellow)
consequence: Both sources give a temperature limit. Neither gives an oxidation rate, so the time to failure above the limit cannot be taken from these sources.
severity: moderate
source: kanthal-nikrothal80
where: Physical properties section, Max continuous operating temperature in air; see also goodfellow-nicr80 Material Overview
- mode: Creep sag under sustained load at high temperature
trigger: A sustained stress at 800 °C or above, for example a wire carrying a tension load in a furnace
consequence: The datasheet gives 15 MPa for 1 % elongation in 1000 h at 800 °C and 4 MPa at 1000 °C, so the allowable sustained stress falls sharply with temperature.
severity: moderate
source: kanthal-nikrothal80
where: Mechanical properties at elevated temperature section, Creep strength rows
side_effects:
- text: Nickel and chromium make up nearly all of the alloy, so the sources classify its raw materials, not the finished wire, as the hazard. Airgas lists nickel and hexavalent chromium compounds on Proposition 65.
affects: Handling of dust and fume from grinding or welding
source: airgas-nickel-sds
where: Regulatory information section, California Proposition 65 line
handling:
- text: The datasheet gives a maximum continuous operating temperature of 1200 °C in air. Use a lower limit for loaded wires, since creep strength at 800 °C is only 15 MPa for 1 % elongation in 1000 h.
source: kanthal-nikrothal80
where: Physical properties section; Mechanical properties at elevated temperature section
mitigations: []
uses:
- application: thermal-control
device: Resistance heating elements
example: Goodfellow lists heating elements in electric furnaces, kilns, toasters, hair dryers and industrial heating equipment. Wikipedia lists hair dryers, heat guns, toasters, kettles and space heaters.
source: goodfellow-nicr80
where: Applications and Advantages section, Heating elements; Wikipedia Uses section
- application: electronics-and-chips
device: Precision wire-wound resistors
example: Goodfellow lists precision wire-wound resistors for power electronics and load banks.
source: goodfellow-nicr80
where: Applications and Advantages section, Resistors
- application: mechanisms
device: Burn-wire release actuator for a CubeSat tie-down
example: A JPL tie-down and release mechanism uses 30 AWG (.010 in diameter) Nichrome wire carrying a 1.6-amp current for about 5 to 10 seconds to cut a Vectran tie-off cable. The brief is dated June 1, 2016.
source: jpl-cubesat-tiedown
where: Description and Nichrome wire size paragraphs
- application: mechanisms
device: Solar panel deployment mechanism
example: Wikipedia says nichrome is used in the solar panel deployment mechanism of spacecraft, citing LightSail-A.
source: wikipedia-nichrome
where: Uses section, Space paragraph
supply:
- subject: Nickel
producers:
- country: Indonesia
share_percent: 66.7
year: 2025
- country: Philippines
share_percent: 6.9
year: 2025
- country: Russia
share_percent: 5.1
year: 2025
- country: Canada
share_percent: 3.6
year: 2025
recycling: 'USGS: nickel recovered from scrap accounted for approximately 60 % of apparent consumption in 2025. Most secondary nickel is stainless-steel scrap.'
substitutes:
- 'USGS: low-nickel, duplex or ultrahigh-chromium stainless steels replace austenitic grades in some uses; titanium alloys can substitute for nickel or nickel-base alloys in corrosive environments.'
source: usgs-mcs2026-nickel
where: World Mine Production and Reserves table, 2025e column (world total 3,900,000 t; shares calculated by Space Mushroom against that printed total); Recycling; Substitutes; Domestic Production and Use (stainless and alloy steel and nickel-containing alloys are more than 85 % of U.S. consumption)
- subject: Chromium
producers:
- country: South Africa
share_percent: 45.1
year: 2025
- country: Turkey
share_percent: 17.6
year: 2025
- country: Kazakhstan
share_percent: 13.7
year: 2025
recycling: 'USGS: recycled chromium in reported stainless-steel scrap receipts accounted for 21 % of supply in 2025.'
substitutes:
- 'USGS: chromium has no substitute in stainless steel or in superalloys.'
source: usgs-mcs2026-chromium
where: World Mine Production and Reserves table, 2025e column (world total 51,000 thousand t; shares calculated by Space Mushroom against that printed total; Kazakhstan value is estimated by USGS); Recycling; Substitutes; Net import reliance 79 % of apparent consumption in 2025e
documents:
- title: 'Bob Martin Co.: 80/20 Nichrome Wire product page (ASTM-B-344, UNS N06003)'
type: datasheet
url: https://www.bobmartinco.com/product/nichromenichrome-and-resistance-alloys/
- title: Kanthal Nikrothal 80 wire datasheet (updated 2024-09-05)
type: datasheet
url: https://kanthal.com/en/products/datasheets/material-datasheets/wire/resistance-heating-wire-and-resistance-wire/nikrothal-80
- title: 'Goodfellow: Nickel/Chromium Ni80/Cr20 wire material information'
type: datasheet
url: https://www.goodfellow.com/usa/resources/nickel-chromium-ni80-cr20-wire-material-information/
- title: 'Wikipedia: Nichrome'
type: database
url: https://en.wikipedia.org/wiki/Nichrome
- title: 'Studer SA: 2.4869 Resistance alloy NiCr 80-20 / N06003'
type: datasheet
url: https://www.studersa.com/en/materials/24869-resistance-alloy-nicr-80-20-n06003;144
- title: 'NASA JPL: Launch Tie-Down and Release Mechanism for CubeSat Spacecraft (Tech Briefs NPO-49969, June 1, 2016)'
type: report
url: https://www.techbriefs.com/component/content/article/24810-npo-49969
year: 2016
- title: 'USGS Mineral Commodity Summaries 2026: Nickel'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-nickel.pdf
year: 2026
- title: 'USGS Mineral Commodity Summaries 2026: Chromium'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-chromium.pdf
year: 2026
- title: Airgas Nickel Wire and Rod safety data sheet, SDS number 011-Ni Wire and Rod (approval 2-1-2016)
type: sds
url: https://www.airgas.com/msds/005727.pdf
year: 2016
gaps:
- Hardness, emissivity and creep strength are listed under non-canonical names (hardness_vickers, emissivity, creep_strength_1pct_1000h) because the canonical property file has no entry for them.
- Strength values are for wire of 1.0 mm and 4.0 mm diameter as the datasheet prints them; the temper or condition of the wire is not stated.
- No CAS number was recorded for the alloy. The search results gave 11106-97-1 for a nickel-chromium product, but no fetched page printed it for this alloy.
- 'Hazard classification: Fisher Scientific and Thomas Scientific listings of 80/20 nickel-chromium wire carry H317 and H351 in search snippets, but the Fisher page did not load, so these codes are not recorded. The Airgas sheet classifies its nickel wire as Not Classified. PubChem could not be read in this run.'
- 'Critical-mineral list status for nickel and chromium: the USGS 2026 nickel and chromium summaries were read and do not name a critical-minerals list in the text extracted, so no list entry is recorded.'
- 'Corrosion: no sulphur, chloride, humidity or vacuum attack data were found. No corrosion rate in micrometres per year was found.'
- Outgassing, atomic-oxygen and radiation effects on NiCr wire were not looked up, and no NASA outgassing value was found.
- Reliable mechanical values for the annealed or as-drawn temper were not found, because the Bob Martin and Ulbrich pages gave no property values and the Ulbrich PDF did not load.
- The Ulbrich and NiWire datasheets (cloud-hosted PDFs) could not be read in this run.
- 'Fe content: the Kanthal page prints an iron limit of Fe 1.0 max on request in one place and a table value of 2.0 max elsewhere, so the iron limit is left out of the composition.'
- Atomic weights of nickel and chromium were not read from a fetched page, so the recipe parts carry shares only.
sources:
bobmartin-8020:
title: 80/20 Nichrome Wire and Nichrome and resistance alloys (Bob Martin Co.)
url: https://www.bobmartinco.com/product/nichromenichrome-and-resistance-alloys/
kind: web
license: Supplier product page (cited, not reproduced)
kanthal-nikrothal80:
title: Nikrothal 80 wire material datasheet (Kanthal), updated 2024-09-05
url: https://kanthal.com/en/products/datasheets/material-datasheets/wire/resistance-heating-wire-and-resistance-wire/nikrothal-80
year: 2024
kind: datasheet
license: Manufacturer datasheet (cited, not reproduced)
goodfellow-nicr80:
title: 'Nickel/Chromium Ni80/Cr20 Wire: material information (Goodfellow)'
url: https://www.goodfellow.com/usa/resources/nickel-chromium-ni80-cr20-wire-material-information/
kind: web
license: Supplier web page (cited, not reproduced)
wikipedia-nichrome:
title: Nichrome (Wikipedia)
url: https://en.wikipedia.org/wiki/Nichrome
year: 2026
kind: web
license: CC BY-SA 4.0 (cited, not reproduced)
studersa-24869:
title: 2.4869 Resistance alloy NiCr 80-20 / N06003 (Studer SA)
url: https://www.studersa.com/en/materials/24869-resistance-alloy-nicr-80-20-n06003;144
kind: web
license: Supplier web page (cited, not reproduced)
jpl-cubesat-tiedown:
title: Launch Tie-Down and Release Mechanism for CubeSat Spacecraft (NASA JPL, Tech Briefs NPO-49969)
url: https://www.techbriefs.com/component/content/article/24810-npo-49969
year: 2016
kind: report
license: NASA JPL tech brief reprinted by Tech Briefs (cited, not reproduced)
usgs-mcs2026-nickel:
title: Mineral Commodity Summaries 2026, Nickel
id: USGS MCS 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-nickel.pdf
year: 2026
kind: report
license: public domain (USGS)
usgs-mcs2026-chromium:
title: Mineral Commodity Summaries 2026, Chromium
id: USGS MCS 2026
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-chromium.pdf
year: 2026
kind: report
license: public domain (USGS)
airgas-nickel-sds:
title: Safety Data Sheet, Nickel Wire and Rod, SDS number 011-Ni Wire and Rod (Airgas)
url: https://www.airgas.com/msds/005727.pdf
year: 2016
kind: datasheet
license: Supplier safety data sheet (cited, not reproduced)
license: CC-BY-4.0
updated: '2026-10-26'
review:
status: draft
method: assistant
checked_values: 21
unreachable: 4
caveats: 5
note: 'Values were read by an AI assistant on 2026-10-26 from the pages named in each entry. Kanthal values are from the manufacturer datasheet for Nikrothal 80. Goodfellow values are approximate and are stated as approximate on the page. Unreachable in this run: PubChem, the Fisher Scientific product page, the Ulbrich PDF and the NiWire PDF. Caveats: the strength values are from wire of two diameters with no temper stated; the 8.4 g/cm3 density and 1.08 to 1.12 µΩ·m resistivity range are approximate supplier values; the nickel and chromium shares are calculated from printed world totals; the Airgas sheet is for a nickel wire and rod product, not the alloy itself.'
story:
risk_groups:
- title: For people
lead: The alloy is about 80 % nickel and 20 % chromium. The sources do not agree on its hazard classification, so the raw materials are the better guide.
level: 1
verdict: Mixed classification
points:
- label: Supplier classification
line: The Airgas nickel wire and rod sheet is classified as Not Classified under GHS and has no signal word. Other suppliers' listings of 80/20 nickel-chromium wire, seen only in search snippets, carry H317 and H351.
- label: Proposition 65
line: The same Airgas sheet lists nickel and hexavalent chromium compounds as carcinogens under California Proposition 65.
- title: If it fails
lead: The failure routes in the sources are temperature and load. The datasheet gives limits but no failure rates.
points:
- label: Overheating
line: Kanthal gives 1200 °C as the continuous limit in air. Goodfellow gives an oxidation limit of 1150 °C. Neither source gives a time to failure above these limits.
- label: Creep
line: At 800 °C the datasheet gives 15 MPa for 1 % elongation in 1000 h, and at 1000 °C it gives 4 MPa.
- title: Handling and storage
points:
- label: Keep it below the limit
line: Kanthal gives 1200 °C as the maximum continuous operating temperature in air. Keep loaded wires below that and well below it when they carry tension.
why: Nichrome is a heating alloy. It combines high electrical resistance with a protective chromium oxide scale, so it can carry current and turn it into heat in air at high temperature. Kanthal's Nikrothal 80 wire has a resistivity of 1.09 Ohm mm2/m at 20 °C, a melting point of 1400 °C and a continuous limit of 1200 °C in air. It is found in heating elements, in precision resistors, and in burn-wire release mechanisms on CubeSats. Its weak points are its low thermal conductivity, 15 W/(m·K) at 20 °C, and its loss of strength at temperature.
uses:
- where: Heating elements
line: Heating elements are the main use. Goodfellow lists electric furnaces, kilns, toasters, hair dryers and industrial heating equipment, and Wikipedia adds kettles, heat guns and space heaters.
- where: Burn-wire releases in CubeSats
line: A JPL tie-down and release mechanism uses 30 AWG nichrome wire to cut a Vectran cable. The source gives a current of 1.6 A applied for about 5 to 10 seconds.
- where: Solar panel deployment
line: Wikipedia says nichrome is used in the solar panel deployment mechanism of spacecraft, citing LightSail-A.
can_do:
- label: Carry current as a heater
value: 1.09 Ohm mm2/m
benchmark: electrical_resistivity
line: The electrical resistivity of Nikrothal 80 is 1.09 Ohm mm2/m at 20 °C, and the Goodfellow range is 1.08 to 1.12 µΩ·m at room temperature.
- label: Stay solid when hot
value: 1400 °C melting point
benchmark: melting_point
line: The melting point is 1400 °C. The continuous operating limit in air is 1200 °C.
- label: Stay light
value: 8.30 g/cm3
benchmark: density
line: Density is 8.30 g/cm3 in the Kanthal datasheet, and about 8.4 g/cm3 in the Goodfellow page.
- label: Strength in fine wire
value: 810 MPa tensile
benchmark: ultimate_tensile_strength
line: In 1.0 mm wire the datasheet gives 810 MPa tensile strength, 420 MPa yield and 30 % elongation at room temperature.
compare: 'This profile has no second heating alloy read in the same run, so the compare rows use nichrome''s own figures: resistivity, continuous temperature limit and thermal conductivity. Read them as nichrome''s values, not as a ranking against another metal.'
compare_rows:
- label: Electrical resistivity
benchmark: electrical_resistivity
- label: Max continuous temperature
benchmark: max_service_temp
- label: Thermal conductivity
benchmark: thermal_conductivity
handling:
- Keep continuous service at or below 1200 °C in air (Kanthal).
- 'Derate for tension at temperature: 15 MPa gives 1 % creep in 1000 h at 800 °C.'
- Treat dust and fume from grinding or welding as containing nickel and chromium compounds (Airgas Proposition 65 listing).
good_for:
- 'Heating elements: 1.09 Ohm mm2/m resistivity and a continuous limit of 1200 °C in air (Kanthal).'
- 'Oxidation resistance: a chromium oxide scale resists oxidation up to about 1150 °C (Goodfellow).'
- 'Fine wire at room temperature: 810 MPa tensile strength and 30 % elongation for 1.0 mm wire (Kanthal).'
watch_out:
- 'Creep: 15 MPa for 1 % elongation in 1000 h at 800 °C, and 4 MPa at 1000 °C.'
- 'Low thermal conductivity: 15 W/(m·K) at 20 °C.'
- 'Hazard classification varies by supplier: Airgas classifies its nickel wire as Not Classified.'
- No corrosion rate, outgassing or radiation data were found.
verdict: Nichrome 80/20 is the standard heating alloy, with a resistivity of 1.09 Ohm mm2/m, a 1400 °C melting point and a 1200 °C continuous limit in air. It is a good choice for a heater, but its strength falls sharply at 800 °C and above, and the profile has no corrosion-rate, outgassing or radiation values.
recipe:
line: Nichrome is a two-element alloy of nickel and chromium, about 80 % nickel and 20 % chromium by mass (Wikipedia, Goodfellow and Studer SA). Kanthal's datasheet gives the chromium range as 19.0 to 21.0 %, with nickel as the balance.
parts:
- name: Nickel
symbol: Ni
share_percent: 80
role: The matrix of the alloy. The balance of the Kanthal composition is nickel.
- name: Chromium
symbol: Cr
share_percent: 20
role: Forms the protective chromium oxide (Cr2O3) scale that resists oxidation in air (Goodfellow).
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.
| # | Source | Type | Year | Used for |
|---|---|---|---|---|
| 80/20 Nichrome Wire and Nichrome and resistance alloys (Bob Martin Co.) | web | 0 values | ||
| Nikrothal 80 wire material datasheet (Kanthal), updated 2024-09-05 | datasheet | 2024 | 23 values | |
| Nickel/Chromium Ni80/Cr20 Wire: material information (Goodfellow) | web | 6 values | ||
| Nichrome (Wikipedia) | web | 2026 | 1 value | |
| 2.4869 Resistance alloy NiCr 80-20 / N06003 (Studer SA) | web | 0 values | ||
| Launch Tie-Down and Release Mechanism for CubeSat Spacecraft (NASA JPL, Tech Briefs NPO-49969) | report | 2016 | 1 value | |
| Mineral Commodity Summaries 2026, Nickel | report | 2026 | 1 value | |
| Mineral Commodity Summaries 2026, Chromium | report | 2026 | 1 value | |