Cobalt Co
Co (element, atomic number 27) · CAS 7440-48-4
Cobalt is the element Co (atomic number 27), a hard, ferromagnetic transition metal.
Evidence level
2 of 5
Lab-measured
- 0Predicted only. No one has made it, or no measurement exists.
- 1Calculated. Only calculated or predicted values from sources.
- 2Lab-measured. Measured properties with their conditions stated.
- 3Space-relevant tests. Measured in conditions relevant to space, such as vacuum or atomic oxygen.
- 4Ground-qualified. Qualified for an application on the ground.
- 5Flown or field-proven. Flight or field results exist.
Carry heat
100 W/(m·K)
Stay magnetic when hot
1115 °C Curie temperature
Weight
8.90 g/cm3
Melt
1495 °C melting point
Strength in two tempers (foil)
1135 MPa hard, 760 MPa soft
Recipe, share of the weight
- Co 100.0%Cobalt
Best for
Hot magnetic and load-bearing alloys: a Curie temperature of 1115 °C and a melting point of 1495 °C in the pure metal, with cobalt-base superalloys for aircraft gas turbines
Weakest at
Supply and fine powder: Congo (Kinshasa) mined an estimated 73 % of world cobalt in 2025, and finely divided cobalt can ignite in air
Risk at a glance
- People Moderate. Carcinogen and sensitiser under EU rules
- If it fails High. Pyrophoric fine powder or dust
- Corrosion Severe. Cobalt dissolves in dilute hydrochloric, sulfuric and nitric acids.
Quick facts: Co
| Property | Value | Basis |
|---|---|---|
| Density | 8.9 g/cm³ | 2 sourced values across conditions |
| Tensile strength | 760 to 1,135 MPa | 2 sourced values across conditions |
| Young's modulus | 209 to 211 GPa | 2 sourced values across conditions |
| Thermal conductivity | 100 W/(m·K) | 1 sourced value |
| Thermal expansion (CTE) | 12.9 ppm/K | 1 sourced value |
| Melting point | 1,495 °C | 1 sourced value |
| Specific heat | 456 J/(kg·K) | 1 sourced value |
| Electrical resistivity | 6.3e-8 Ω·m | 2 sourced values across conditions |
What is the density of Cobalt?
Cobalt has a density of 8.9 g/cm³. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is the thermal conductivity of Cobalt?
Cobalt has a thermal conductivity of 100 W/(m·K). The source and test conditions are listed in the properties table on this page.
What is the coefficient of thermal expansion of Cobalt?
Cobalt has a coefficient of thermal expansion of 12.9 ppm/K. The source and test conditions are listed in the properties table on this page.
What is the melting point of Cobalt?
Cobalt has a melting point of 1,495 °C. The source and test conditions are listed in the properties table on this page.
What is the tensile strength of Cobalt?
Cobalt has a tensile strength of 760 to 1,135 MPa. The range covers 2 sourced values across the tempers, forms and test conditions the sources report; room-temperature values are used where a source states a temperature.
What is Cobalt used for?
Uses recorded in the sources include Cathode metal in lithium-ion cells (lithium cobalt oxide and nickel-manganese-cobalt cathodes); Cobalt-base superalloys for aircraft gas turbine engines; Connectors, thermal switches and microsensors in aerospace electronics.
Why it exists
Cobalt is a hard, ferromagnetic metal. Goodfellow gives its density as 8.90 g/cm3 at 20 °C and its melting point as 1495 °C, and it stays ferromagnetic up to its Curie temperature of 1115 °C. Its thermal conductivity is 100 W/(m·K) in the Goodfellow rod data. It is used mainly as an alloy element: superalloys took 51 % of US cobalt use in 2025, mainly for aircraft gas turbine engines (USGS), and the cobalt content of lithium-ion batteries is the leading global use. Congo (Kinshasa) mined an estimated 73 % of world cobalt in 2025.
Where it's used
Batteries
The cobalt content of lithium-ion batteries is the leading global use of cobalt, according to the USGS. Cobalt-free cells that use iron and phosphorus held a significant share of the market in China.
Aircraft engines
In the United States, superalloys took 51 % of cobalt use in 2025, mainly for aircraft gas turbine engines. Goodfellow adds nozzle guide vanes, combustion liners and first-stage turbine blades as cobalt-base alloy parts.
Satellite electronics
Wikipedia says cobalt alloys are used in connectors, thermal switches and microsensors that must endure extreme temperatures, vibration and radiation, conditions typical in satellites.
Magnets and actuators
Samarium-cobalt magnets outperform NdFeB above about 150 °C and in corrosive environments, which Goodfellow gives as the reason for their use in high-temperature motors, sensors and aerospace actuators.
Recipe
Co (element, atomic number 27); unalloyed cobalt metal, hexagonal close-packed (alpha-Co) below 417 °C and face-centred cubic (beta-Co) above
Cobalt is a single-element metal, Co, with a hexagonal close-packed structure below 417 °C and a face-centred cubic structure above it (Goodfellow). Today it is usually produced as a by-product of copper and nickel mining, and the free element is made by reductive smelting (Wikipedia).
| Ingredient | Atoms per unit | Share of the weight | What it does |
|---|---|---|---|
| Cobalt Co | 1 | 100.0% | The whole material: unalloyed cobalt metal. The NIST standard atomic weight is 58.933 194(4). |
Weight shares are calculated from standard atomic weights.
What it can do
Carry heat
100 W/(m·K)
measured
The Goodfellow rod data gives 100 W/(m·K) for 0 to 100 °C. A reseller listing gives 1.0 W/(cm·K) at 298.2 K, which is the same order of magnitude.
Stay magnetic when hot
1115 °C Curie temperature
measured
Cobalt stops being ferromagnetic only at its Curie temperature of 1115 °C, which Goodfellow describes as the highest of any ferromagnetic element.
Weight
8.90 g/cm3
measured
The density is 8.90 g/cm3 at 20 °C on the Goodfellow metal page, and 8.9 g/cm3 on the rod page.
Melt
1495 °C melting point
measured
The melting point is 1495 °C (1768 K) on the Goodfellow page. PubChem prints the boiling point as 2,927 °C in its HSDB entry, against 2870 °C on the Goodfellow page.
Strength in two tempers (foil)
1135 MPa hard, 760 MPa soft
measured
A 0.025 mm cobalt foil of 99.8 % purity has tensile strength 1135 MPa in the hard temper and 760 MPa in the soft temper, with Vickers hardness 320 and 170.
Expansion
12.5 ppm/K
measured
The coefficient of thermal expansion is 12.5 ppm/K from 0 to 100 °C on the Goodfellow rod page, and 12.9 ppm/K at 20 °C in Wikipedia.
How it compares
Goodfellow describes the density of cobalt as intermediate between those of iron and nickel, and its thermal conductivity as similar to both. Iron and nickel are similar metals, so read the table rows as examples of the same class, not as a ranking.
The same measurements for each material, so you can compare them. Each row names the key condition under the value; the full conditions and methods are in the numbered notes under Technical details. Compare every grade in the family.
| Measurement | Co |
|---|---|
| Thermal behavior and safety | |
| Melting point, high-purity cobaltValue printed in a supplier material data table | 1495 °C |
| Thermal conductivity, high-purity cobalt rod (0 to 100 °C) | 100 W/(m·K)4 |
| Thermal conductivity, cobalt rod at 298.2 K (reseller listing) | 1 W/(cm·K)5 |
| Specific heat capacity, high-purity cobalt rod at 25 °C | 456 J/(kg·K)6 |
| Specific heat capacity, cobalt at 15 to 100 °CValue printed in a database record (HSDB entry) | 0.442 J/g °C |
| Latent heat of fusion, high-purity cobalt rod | 263 J/g15 |
| Physical and electrical | |
| Density at 20 °C, high-purity cobalt metalValue printed in a supplier material data table | 8.9 g/cm³ |
| Density at 20 °C, high-purity cobalt rod | 8.9 g/cm³1 |
| Electrical resistivity at 20 °C, high-purity cobalt metalValue printed in a supplier material data table | 62.4 nΩ·m |
| Electrical resistivity at 20 °C, high-purity cobalt rod | 6.34 µΩ·cm3 |
| Vickers hardness, cobalt foil 0.025 mm thick, hard temper | 320 kgf/mm213 |
| Vickers hardness, cobalt foil 0.025 mm thick, soft temper | 170 kgf/mm214 |
| Temperature behavior | |
| Curie temperature, cobaltValue printed in an encyclopaedia article | 1115 °C |
| Transformation from hcp to fcc, cobaltValue printed in a database record (HSDB entry) | 417 °C |
| Other measurements | |
| Boiling point, high-purity cobaltValue printed in a supplier material data table | 2870 °C |
| Boiling point, elemental cobalt (HSDB entry) | 2927 °C2 |
| Coefficient of thermal expansion, high-purity cobalt rod (0 to 100 °C) | 12.5 ppm/K7 |
| Coefficient of thermal expansion, cobalt at 20 °CValue printed in an encyclopaedia infobox | 12.9 ppm/K |
| Young's modulus, high-purity cobalt metalValue printed in a supplier material data table | 209 GPa |
| Tensile modulus, cobalt foil 0.025 mm thick | 211 GPa8 |
| Bulk modulus, cobalt foil 0.025 mm thick | 181.5 GPa9 |
| Poisson's ratio, cobaltValue printed in an encyclopaedia infobox | 0.31 - |
| Poisson's ratio, cobalt foil 0.025 mm thick | 0.32 -10 |
| Tensile strength, cobalt foil 0.025 mm thick, hard temper | 1135 MPa11 |
| Tensile strength, cobalt foil 0.025 mm thick, soft temper | 760 MPa12 |
| Saturation magnetization, cobaltValue printed on a supplier material page | 1.42 T |
Why choose it, and why not
Good for
- High-temperature magnets: a Curie temperature of 1115 °C, and samarium-cobalt magnets that outperform NdFeB above about 150 °C (Goodfellow).
- Hot alloys: cobalt-base superalloys for aircraft gas turbine engines (USGS).
- Battery cathodes: the leading global use of cobalt, according to the USGS.
Watch out for
- Supply is concentrated: Congo (Kinshasa) mined an estimated 73 % of world cobalt in 2025, and export quotas run to 96,600 t per year in 2026 and 2027.
- The EU classification includes H350 (may cause cancer) and H317 (allergic skin reaction).
- Fine powder can ignite in air, and acid attack releases hydrogen.
- No atomic-oxygen, outgassing or radiation data for pure cobalt in space was found.
Cobalt is a dense, hard, high-temperature ferromagnetic metal with a melting point of 1495 °C and a Curie temperature of 1115 °C. Its main roles are as an alloy element in magnets, superalloys and battery cathodes, and its supply is concentrated in Congo (Kinshasa). The EU classifies the metal as a carcinogen and a sensitiser, and fine powder is pyrophoric. The profile has no space outgassing, atomic-oxygen or designation data for pure cobalt.
Technical details
For scientists and researchers. Everything above comes from the record below: every number with its method, its conditions and its source.
Notes
The method, full conditions and any caveat for the numbered rows above.
| # | Measurement | Method | Conditions | Caveat |
|---|---|---|---|---|
| 1 | Density at 20 °C, high-purity cobalt rod | Value printed in a supplier physical properties table | temperature 20 °Cform solid rod, high-purity (Goodfellow rod page) | — |
| 2 | Boiling point, elemental cobalt (HSDB entry) | Experimental value listed in PubChem, from the Hazardous Substances Data Bank (HSDB) entry | pressure 760 mmHgform elemental cobalt | PubChem also lists 2870 °C from an ICSC entry, so the boiling point differs by 57 °C between sources. |
| 3 | Electrical resistivity at 20 °C, high-purity cobalt rod | Value printed in a supplier electrical properties table | temperature 20 °Cform solid rod, high-purity | The metal page prints 62.4 nΩ·m for the same quantity, which is 6.24 µΩ·cm, 0.1 µΩ·cm below this rod value. |
| 4 | Thermal conductivity, high-purity cobalt rod (0 to 100 °C) | Value printed in a supplier thermal properties table | temperature 0 to 100 °Cform solid rod, high-purityunit in source W m-1 K-1 | — |
| 5 | Thermal conductivity, cobalt rod at 298.2 K (reseller listing) | Value printed on a reseller's product specification list | temperature 298.2 Kform cobalt rod, product listing | — |
| 6 | Specific heat capacity, high-purity cobalt rod at 25 °C | Value printed in a supplier thermal properties table | temperature 25 °Cform solid rod, high-purity | — |
| 7 | Coefficient of thermal expansion, high-purity cobalt rod (0 to 100 °C) | Value printed in a supplier thermal properties table | temperature 0 to 100 °Cform solid rod, high-purityunit in source x10-6 K-1 | — |
| 8 | Tensile modulus, cobalt foil 0.025 mm thick | Value printed in a supplier mechanical properties table | form foil, 0.025 mm thick, 99.8 % puritytemper not stated; the hard and soft rows both print 211 | — |
| 9 | Bulk modulus, cobalt foil 0.025 mm thick | Value printed in a supplier mechanical properties table | form foil, 0.025 mm thick, 99.8 % puritytemper not stated; the hard and soft rows both print 181.5 | — |
| 10 | Poisson's ratio, cobalt foil 0.025 mm thick | Value printed in a supplier mechanical properties table | form foil, 0.025 mm thick, 99.8 % puritytemper not stated; the hard and soft rows both print 0.32 | — |
| 11 | Tensile strength, cobalt foil 0.025 mm thick, hard temper | Value printed in a supplier mechanical properties table | form foil, 0.025 mm thick, 99.8 % puritytemper hard | — |
| 12 | Tensile strength, cobalt foil 0.025 mm thick, soft temper | Value printed in a supplier mechanical properties table | form foil, 0.025 mm thick, 99.8 % puritytemper soft | — |
| 13 | Vickers hardness, cobalt foil 0.025 mm thick, hard temper | Value printed in a supplier mechanical properties table | form foil, 0.025 mm thick, 99.8 % puritytemper hardload not stated | — |
| 14 | Vickers hardness, cobalt foil 0.025 mm thick, soft temper | Value printed in a supplier mechanical properties table | form foil, 0.025 mm thick, 99.8 % puritytemper softload not stated | — |
| 15 | Latent heat of fusion, high-purity cobalt rod | Value printed in a supplier thermal properties table | form solid rod, high-purity | — |
Corrosion and compatibility
What happens when it meets other materials and environments.
| Environment | Concern | What happens |
|---|---|---|
| Air at room temperature | moderate | Cobalt oxidises slowly in air and forms a thin oxide layer that is less protective than chromium oxide.1 |
| Air, as a stability statement | not rated | A database record says cobalt corrodes readily in air.2 |
| Dilute mineral acids (hydrochloric, sulfuric, nitric) | severe | Cobalt dissolves in dilute hydrochloric, sulfuric and nitric acids.3 |
| Alkalis and many organic acids | low | Cobalt resists alkalis and many organic acids at room temperature.4 |
| # | Environment | Details | Test conditions |
|---|---|---|---|
| 1 | Air at room temperature | Goodfellow says cobalt oxidises slowly in air at room temperature. The mixed Co3O4 spinel layer slows further oxidation but is less protective than Cr2O3, so chromium and aluminium additions improve oxidation resistance. The rating on the page is moderate. | basis supplier statement; no oxide thickness, rate or test duration printedtemperature room temperature |
| 2 | Air, as a stability statement | PubChem's record, from the Hazardous Substances Data Bank, gives 'Corrodes readily in air' under stability and shelf life. No test conditions or rate are printed. | basis database statement; no test conditions printed |
| 3 | Dilute mineral acids (hydrochloric, sulfuric, nitric) | Goodfellow lists cobalt as dissolving in dilute HCl, H2SO4 and HNO3, and as reacting with mineral acids to form Co2+ salts. Concentrated nitric acid passivates it, and aqua regia dissolves it rapidly. | basis supplier statements; acid concentrations and temperatures for the dilute acids are not printed |
| 4 | Alkalis and many organic acids | Goodfellow lists cobalt as resistant to alkalis, and to acetic acid and many organic acids at room temperature. | basis supplier statement; no concentration printedtemperature room temperature |
Risks and side effects
Hazards to people, what happens when a cell overheats, and how the material is handled and stored.
For people
The EU harmonised classification lists cobalt metal as a skin and respiratory sensitiser, suspected of causing genetic defects, and as a substance that may cause cancer. ECHA notifications differ on the rest.
- Harmonised classification
- PubChem prints the EU classification under Regulation (EC) No 1272/2008: H317, H334, H341 and H350, signal word Danger.
- Notifications
- Of 2,768 company reports to ECHA, one says cobalt does not meet GHS criteria. Among reports that gave codes, H317 is given by more than 99.9 %, H302 by 65.2 % and H330 by 23.4 %.
If it fails
The failure routes printed in the sources are fire from fine powder and acid attack with hydrogen release. No space exposure data for pure cobalt was found.
- Fine powder
- Finely divided cobalt can ignite in air, and dust can form explosive mixtures in air.
- Acid
- Dilute hydrochloric, sulfuric and nitric acids dissolve cobalt, and the reaction releases flammable and explosive hydrogen.
Handling and storage
- Dust limits
- The OSHA limit for cobalt metal dust and fume is 0.1 mg/m3 and the NIOSH limit is 0.05 mg/m3, both as Co.
- Keep fine cobalt apart
- Keep fine cobalt away from air, oxidising agents, acetylene and ammonium nitrate.
Test details
The original wording and numbers from the sources, for readers who want them.
Failure risks
| Failure | Trigger and consequence |
|---|---|
| Pyrophoric fine powder or dusthigh severity | Finely divided cobalt, including powder reduced from its oxides, exposed to air, acetylene or oxidising agentsPubChem (HSDB) says only certain forms of cobalt metal are pyrophoric, and very fine cobalt dust reduced in hydrogen can catch fire at room temperature in air. Dust can form explosive mixtures in air, and fused ammonium nitrate with powdered metals can react violently. |
| Acid attack with hydrogen releasemoderate severity | Contact with mineral acids such as hydrochloric or sulfuric acidCobalt reacts with mineral acids to form Co2+ salts, and the reaction generates flammable and explosive hydrogen gas (HSDB). |
| Surface oxidation in airlow severity | Long exposure to air at room temperatureCobalt oxidises slowly to a Co3O4 layer, which is less protective than chromium oxide. The source gives no oxide thickness or rate. |
Side effects on surrounding parts
| Affects | Effect |
|---|---|
| Radiation dose and contamination from cobalt in reactor components and in radiotherapy sources | Cobalt-59 captures neutrons in nuclear reactors to form cobalt-60, which has a half-life of 5.27 years and emits gamma rays at 1.17 and 1.33 MeV. Cobalt-60 is also a corrosion product activated in reactor coolant circuits. |
Handling and storage
- Occupational limits for cobalt metal dust and fume, as Co: OSHA permissible exposure limit 0.1 mg/m3 as an 8-hour time-weighted average, and NIOSH recommended exposure limit 0.05 mg/m3 as a 10-hour time-weighted average.
- The NIOSH Pocket Guide excerpt in PubChem lists cough, dyspnoea, wheezing, decreased lung function, dermatitis, respiratory hypersensitivity and asthma as symptoms of cobalt metal dust and fume. Target organs are the skin and respiratory system.
- ATSDR lists cancer, skin, blood-forming, liver and respiratory effects as the affected organ systems for cobalt.
- Keep finely divided cobalt away from air, acetylene, oxidising agents and ammonium nitrate. PubChem warns of violent reactions with these.
Supply and geography
How common the raw materials are and where they come from.
Cobalt mine production, 2025
- Top producers (2025)
- Congo (Kinshasa) 73%, Indonesia 14%
Cobalt reserves and resources
Congo (Kinshasa) export controls
United States cobalt use, imports and recycling
- Recycling
- Cobalt content of purchased scrap was 25 % of estimated cobalt consumption in 2025 (USGS).
Cobalt price, US$ per pound
Critical-material status
- Critical mineral lists
- US: listed
Substitutes
- Substitutes
- USGS: cobalt-free lithium-ion cathodes using iron and phosphorus held significant market share in China. In magnets: barium or strontium ferrites, neodymium-iron-boron or nickel-iron alloys. In paints: cerium, iron, lead, manganese or vanadium. In jet engines: nickel-base alloys or ceramics. In cutting and wear-resistant materials: iron, nickel, cermets or ceramics.
Documents
Datasheets, safety data sheets, papers and standards you can open.
Full record
The complete spore, as stored. Free to reuse under CC-BY-4.0. Images keep the licence shown with each one.
Show the full YAML
spore: profile
id: cobalt
spore_version: 0.2
family: cobalt-alloys
name: Cobalt
abbreviation: Co
role: magnet, superalloy and battery metal
category: metals
type: heavy-metals
summary: |
Cobalt is the element Co (atomic number 27), a hard, ferromagnetic transition metal. The unalloyed metal has a density of 8.90 g/cm3 at 20 °C, a melting point of 1495 °C and a Curie temperature of 1115 °C. Goodfellow gives its thermal conductivity as 100 W/(m·K). Most cobalt is used as an alloy element or in compounds: lithium-ion cathodes, cobalt-base superalloys for aircraft gas turbines, and samarium-cobalt magnets. Congo (Kinshasa) mined an estimated 73 % of world cobalt in 2025, and the USGS reports export quotas that replaced a temporary export ban.
best_for: 'Hot magnetic and load-bearing alloys: a Curie temperature of 1115 °C and a melting point of 1495 °C in the pure metal, with cobalt-base superalloys for aircraft gas turbines'
weakest_at: 'Supply and fine powder: Congo (Kinshasa) mined an estimated 73 % of world cobalt in 2025, and finely divided cobalt can ignite in air'
identity:
formula: Co (element, atomic number 27); unalloyed cobalt metal, hexagonal close-packed (alpha-Co) below 417 °C and face-centred cubic (beta-Co) above
cas: 7440-48-4
source: goodfellow-co-metal
where: CAS Number row and Atomic Number row (27) of the Goodfellow high-purity cobalt material page; Crystal Structure row gives hcp below 417 °C and fcc above
tags:
environments: []
stresses:
- extreme-heat
applications:
- batteries
- electronics-and-chips
- mechanisms
- propulsion-and-tanks
properties:
- benchmark: density
label: Density at 20 °C, high-purity cobalt metal
value: 8.9
unit: g/cm3
scope: material
conditions:
temperature: 20 °C
form: high-purity cobalt metal (Goodfellow material page)
method: Value printed in a supplier material data table
status: ground
source: goodfellow-co-metal
where: Physical data table, row Density (20 °C)
- benchmark: density
label: Density at 20 °C, high-purity cobalt rod
value: 8.9
unit: g/cm3
scope: material
conditions:
temperature: 20 °C
form: solid rod, high-purity (Goodfellow rod page)
method: Value printed in a supplier physical properties table
status: ground
source: goodfellow-co-rod
where: Physical Properties table, row Density, 8.9@20°C
- benchmark: melting_point
label: Melting point, high-purity cobalt
value: 1495
unit: °C
scope: material
conditions:
form: high-purity cobalt metal
unit_in_source: 1,495 °C (1,768 K)
method: Value printed in a supplier material data table
status: ground
source: goodfellow-co-metal
where: Physical data table, row Melting Point, 1,495 °C (1,768 K)
- benchmark: boiling_point
label: Boiling point, high-purity cobalt
value: 2870
unit: °C
scope: material
conditions:
unit_in_source: 2,870 °C (3,143 K)
pressure: not stated
method: Value printed in a supplier material data table
status: ground
source: goodfellow-co-metal
where: Physical data table, row Boiling Point, 2,870 °C (3,143 K)
- benchmark: boiling_point
label: Boiling point, elemental cobalt (HSDB entry)
value: 2927
unit: °C
scope: material
conditions:
pressure: 760 mmHg
form: elemental cobalt
method: Experimental value listed in PubChem, from the Hazardous Substances Data Bank (HSDB) entry
status: ground
note: PubChem also lists 2870 °C from an ICSC entry, so the boiling point differs by 57 °C between sources.
source: pubchem-co
where: Experimental Properties, Boiling Point, HSDB entry 2,927 °C
- benchmark: curie_temperature
label: Curie temperature, cobalt
value: 1115
unit: °C
scope: material
conditions:
unit_in_source: 1,115 °C (1,388 K; 2,039 °F)
method: Value printed in an encyclopaedia article
status: ground
source: wikipedia-co
where: Paragraph beginning 'Cobalt is a ferromagnetic metal with a specific gravity of 8.9'
- benchmark: electrical_resistivity
label: Electrical resistivity at 20 °C, high-purity cobalt metal
value: 62.4
unit: nΩ·m
scope: material
conditions:
temperature: 20 °C
form: high-purity cobalt metal
method: Value printed in a supplier material data table
status: ground
source: goodfellow-co-metal
where: Electrical Properties table, row Electrical Resistivity, 62.4 nΩ·m (20 °C)
- benchmark: electrical_resistivity
label: Electrical resistivity at 20 °C, high-purity cobalt rod
value: 6.34
unit: µΩ·cm
scope: material
conditions:
temperature: 20 °C
form: solid rod, high-purity
method: Value printed in a supplier electrical properties table
status: ground
note: The metal page prints 62.4 nΩ·m for the same quantity, which is 6.24 µΩ·cm, 0.1 µΩ·cm below this rod value.
source: goodfellow-co-rod
where: Electrical Properties table, row Electrical resistivity (µOhmcm), 6.34@20°C
- benchmark: thermal_conductivity
label: Thermal conductivity, high-purity cobalt rod (0 to 100 °C)
value: 100
unit: W/(m·K)
scope: material
conditions:
temperature: 0 to 100 °C
form: solid rod, high-purity
unit_in_source: W m-1 K-1
method: Value printed in a supplier thermal properties table
status: ground
source: goodfellow-co-rod
where: Thermal Properties table, row Thermal conductivity, 100@0-100°C
- benchmark: thermal_conductivity
label: Thermal conductivity, cobalt rod at 298.2 K (reseller listing)
value: 1
unit: W/(cm·K)
scope: material
conditions:
temperature: 298.2 K
form: cobalt rod, product listing
method: Value printed on a reseller's product specification list
status: ground
source: fine-metals-co-rod
where: Product specification list, row Thermal Conductivity, 1.0 W/cm/K @ 298.2 K
- benchmark: specific_heat
label: Specific heat capacity, high-purity cobalt rod at 25 °C
value: 456
unit: J/(kg·K)
scope: material
conditions:
temperature: 25 °C
form: solid rod, high-purity
method: Value printed in a supplier thermal properties table
status: ground
source: goodfellow-co-rod
where: Thermal Properties table, row Specific heat, 456@25°C
- benchmark: specific_heat
label: Specific heat capacity, cobalt at 15 to 100 °C
value: 0.442
unit: J/g °C
scope: material
conditions:
temperature: 15 to 100 °C
unit_in_source: J/g °C
method: Value printed in a database record (HSDB entry)
status: ground
source: pubchem-co
where: Experimental Properties, Other Experimental Properties, specific heat entry 0.442 J/g °C (15-100 °C)
- benchmark: cte
label: Coefficient of thermal expansion, high-purity cobalt rod (0 to 100 °C)
value: 12.5
unit: ppm/K
scope: material
conditions:
temperature: 0 to 100 °C
form: solid rod, high-purity
unit_in_source: x10-6 K-1
method: Value printed in a supplier thermal properties table
status: ground
source: goodfellow-co-rod
where: Thermal Properties table, row Coefficient of thermal expansion, 12.5@0-100°C
- benchmark: cte
label: Coefficient of thermal expansion, cobalt at 20 °C
value: 12.9
unit: ppm/K
scope: material
conditions:
temperature: 20 °C
unit_in_source: 12.9 × 10−6/K
method: Value printed in an encyclopaedia infobox
status: ground
source: wikipedia-co
where: Infobox, row Thermal expansion
- benchmark: elastic_modulus
label: Young's modulus, high-purity cobalt metal
value: 209
unit: GPa
scope: material
conditions:
form: high-purity cobalt metal
temperature: not stated
method: Value printed in a supplier material data table
status: ground
source: goodfellow-co-metal
where: Mechanical properties table, row Elastic (Young's) Modulus, 209 GPa
- benchmark: elastic_modulus
label: Tensile modulus, cobalt foil 0.025 mm thick
value: 211
unit: GPa
scope: material
conditions:
form: foil, 0.025 mm thick, 99.8 % purity
temper: not stated; the hard and soft rows both print 211
method: Value printed in a supplier mechanical properties table
status: ground
source: goodfellow-co-foil
where: Mechanical Properties table, row Tensile modulus (GPa)
- benchmark: bulk_modulus
label: Bulk modulus, cobalt foil 0.025 mm thick
value: 181.5
unit: GPa
scope: material
conditions:
form: foil, 0.025 mm thick, 99.8 % purity
temper: not stated; the hard and soft rows both print 181.5
method: Value printed in a supplier mechanical properties table
status: ground
source: goodfellow-co-foil
where: Mechanical Properties table, row Bulk modulus (GPa)
- benchmark: poissons_ratio
label: Poisson's ratio, cobalt
value: 0.31
unit: '-'
scope: material
conditions:
temperature: not stated
method: Value printed in an encyclopaedia infobox
status: ground
source: wikipedia-co
where: Infobox, row Poisson ratio, 0.31
- benchmark: poissons_ratio
label: Poisson's ratio, cobalt foil 0.025 mm thick
value: 0.32
unit: '-'
scope: material
conditions:
form: foil, 0.025 mm thick, 99.8 % purity
temper: not stated; the hard and soft rows both print 0.32
method: Value printed in a supplier mechanical properties table
status: ground
source: goodfellow-co-foil
where: Mechanical Properties table, row Poisson's ratio
- benchmark: ultimate_tensile_strength
label: Tensile strength, cobalt foil 0.025 mm thick, hard temper
value: 1135
unit: MPa
scope: material
conditions:
form: foil, 0.025 mm thick, 99.8 % purity
temper: hard
method: Value printed in a supplier mechanical properties table
status: ground
source: goodfellow-co-foil
where: Mechanical Properties table, row Tensile strength (MPa), material condition Hard
- benchmark: ultimate_tensile_strength
label: Tensile strength, cobalt foil 0.025 mm thick, soft temper
value: 760
unit: MPa
scope: material
conditions:
form: foil, 0.025 mm thick, 99.8 % purity
temper: soft
method: Value printed in a supplier mechanical properties table
status: ground
source: goodfellow-co-foil
where: Mechanical Properties table, row Tensile strength (MPa), material condition Soft
- benchmark: vickers_hardness
label: Vickers hardness, cobalt foil 0.025 mm thick, hard temper
value: 320
unit: kgf/mm2
scope: material
conditions:
form: foil, 0.025 mm thick, 99.8 % purity
temper: hard
load: not stated
method: Value printed in a supplier mechanical properties table
status: ground
source: goodfellow-co-foil
where: Mechanical Properties table, row Hardness Vickers (kgf mm-2), material condition Hard
- benchmark: vickers_hardness
label: Vickers hardness, cobalt foil 0.025 mm thick, soft temper
value: 170
unit: kgf/mm2
scope: material
conditions:
form: foil, 0.025 mm thick, 99.8 % purity
temper: soft
load: not stated
method: Value printed in a supplier mechanical properties table
status: ground
source: goodfellow-co-foil
where: Mechanical Properties table, row Hardness Vickers (kgf mm-2), material condition Soft
- benchmark: saturation_magnetization
label: Saturation magnetization, cobalt
value: 1.42
unit: T
scope: material
conditions:
temperature: not stated
method: Value printed on a supplier material page
status: ground
source: goodfellow-co-metal
where: Magnetic Properties row, 'saturation magnetization 1.42 T'
- benchmark: heat_of_fusion
label: Latent heat of fusion, high-purity cobalt rod
value: 263
unit: J/g
scope: material
conditions:
form: solid rod, high-purity
method: Value printed in a supplier thermal properties table
status: ground
source: goodfellow-co-rod
where: Thermal Properties table, row Latent heat of fusion, 263
- benchmark: phase_transformation_temperature
label: Transformation from hcp to fcc, cobalt
value: 417
unit: °C
scope: material
conditions:
transition: hexagonal close-packed to face-centred cubic
method: Value printed in a database record (HSDB entry)
status: ground
source: pubchem-co
where: 'Experimental Properties, Other Experimental Properties, entry ''Transformation temperature: 417 °C'''
corrosion:
- environment: Air at room temperature
headline: Cobalt oxidises slowly in air and forms a thin oxide layer that is less protective than chromium oxide.
effect: Goodfellow says cobalt oxidises slowly in air at room temperature. The mixed Co3O4 spinel layer slows further oxidation but is less protective than Cr2O3, so chromium and aluminium additions improve oxidation resistance. The rating on the page is moderate.
rating: moderate
conditions:
basis: supplier statement; no oxide thickness, rate or test duration printed
temperature: room temperature
source: goodfellow-co-metal
where: Corrosion Resistance row (Moderate, Co3O4 spinel layer)
- environment: Air, as a stability statement
headline: A database record says cobalt corrodes readily in air.
effect: PubChem's record, from the Hazardous Substances Data Bank, gives 'Corrodes readily in air' under stability and shelf life. No test conditions or rate are printed.
conditions:
basis: database statement; no test conditions printed
source: pubchem-co
where: Experimental Properties, Stability/Shelf Life entry (HSDB)
rating: unknown
- environment: Dilute mineral acids (hydrochloric, sulfuric, nitric)
headline: Cobalt dissolves in dilute hydrochloric, sulfuric and nitric acids.
effect: Goodfellow lists cobalt as dissolving in dilute HCl, H2SO4 and HNO3, and as reacting with mineral acids to form Co2+ salts. Concentrated nitric acid passivates it, and aqua regia dissolves it rapidly.
rating: severe
conditions:
basis: supplier statements; acid concentrations and temperatures for the dilute acids are not printed
source: goodfellow-co-metal
where: Acid Resistance row
- environment: Alkalis and many organic acids
headline: Cobalt resists alkalis and many organic acids at room temperature.
effect: Goodfellow lists cobalt as resistant to alkalis, and to acetic acid and many organic acids at room temperature.
rating: low
conditions:
basis: supplier statement; no concentration printed
temperature: room temperature
source: goodfellow-co-metal
where: Acid Resistance row
risks:
hazards:
- text: The EU harmonised classification under Regulation (EC) No 1272/2008, as printed in PubChem, is H317 (may cause an allergic skin reaction), H334 (may cause allergy or asthma symptoms or breathing difficulties if inhaled), H341 (suspected of causing genetic defects) and H350 (may cause cancer). Signal word Danger. Hazard classes Carc. 1B, Muta. 2, Repr. 1B and Resp. Sens. 1.
ghs:
- H317
- H334
- H341
- H350
source: pubchem-co
where: GHS Classification, Regulation (EC) No 1272/2008 entry, and Hazard Classes and Categories
- text: PubChem's ECHA C&L summary is aggregated from 2,768 company reports. One report says cobalt does not meet GHS criteria. Notified codes are H302 (65.2 %), H317 (above 99.9 %), H319 (40.8 %) and H330 (23.4 %), with signal word Danger.
ghs:
- H302
- H317
- H319
- H330
source: pubchem-co
where: GHS Classification, ECHA C&L Notifications Summary
failure_risks:
- mode: Pyrophoric fine powder or dust
trigger: Finely divided cobalt, including powder reduced from its oxides, exposed to air, acetylene or oxidising agents
consequence: PubChem (HSDB) says only certain forms of cobalt metal are pyrophoric, and very fine cobalt dust reduced in hydrogen can catch fire at room temperature in air. Dust can form explosive mixtures in air, and fused ammonium nitrate with powdered metals can react violently.
severity: high
source: pubchem-co
where: Fire Potential, Physical Dangers and Stability and Reactivity entries (HSDB)
- mode: Acid attack with hydrogen release
trigger: Contact with mineral acids such as hydrochloric or sulfuric acid
consequence: Cobalt reacts with mineral acids to form Co2+ salts, and the reaction generates flammable and explosive hydrogen gas (HSDB).
severity: moderate
source: pubchem-co
where: Hazardous Reactivities and Incompatibilities entries (HSDB)
- mode: Surface oxidation in air
trigger: Long exposure to air at room temperature
consequence: Cobalt oxidises slowly to a Co3O4 layer, which is less protective than chromium oxide. The source gives no oxide thickness or rate.
severity: low
source: goodfellow-co-metal
where: Corrosion Resistance row
side_effects:
- text: Cobalt-59 captures neutrons in nuclear reactors to form cobalt-60, which has a half-life of 5.27 years and emits gamma rays at 1.17 and 1.33 MeV. Cobalt-60 is also a corrosion product activated in reactor coolant circuits.
affects: Radiation dose and contamination from cobalt in reactor components and in radiotherapy sources
source: goodfellow-co-metal
where: Isotopes table, 60Co entry
handling:
- text: 'Occupational limits for cobalt metal dust and fume, as Co: OSHA permissible exposure limit 0.1 mg/m3 as an 8-hour time-weighted average, and NIOSH recommended exposure limit 0.05 mg/m3 as a 10-hour time-weighted average.'
source: pubchem-co
where: Safety and Hazard Properties, OSHA Standards and NIOSH Recommendations entries
- text: The NIOSH Pocket Guide excerpt in PubChem lists cough, dyspnoea, wheezing, decreased lung function, dermatitis, respiratory hypersensitivity and asthma as symptoms of cobalt metal dust and fume. Target organs are the skin and respiratory system.
source: pubchem-co
where: Health Hazards, excerpt from NIOSH Pocket Guide (2024)
- text: ATSDR lists cancer, skin, blood-forming, liver and respiratory effects as the affected organ systems for cobalt.
source: atsdr-cobalt
where: Affected Organ Systems line
- text: Keep finely divided cobalt away from air, acetylene, oxidising agents and ammonium nitrate. PubChem warns of violent reactions with these.
source: pubchem-co
where: Reactivity Profile and Hazardous Reactivities and Incompatibilities entries (HSDB)
mitigations: []
uses:
- application: batteries
device: Cathode metal in lithium-ion cells (lithium cobalt oxide and nickel-manganese-cobalt cathodes)
example: USGS says the cobalt content of lithium-ion batteries is the leading global use of cobalt. Cobalt-free cells using iron and phosphorus held a significant market share in China.
source: usgs-mcs2026-cobalt
where: Substitutes paragraph
- application: propulsion-and-tanks
device: Cobalt-base superalloys for aircraft gas turbine engines
example: USGS says superalloys took 51 % of cobalt consumed in the United States in 2025, mainly for aircraft gas turbine engines. Goodfellow adds nozzle guide vanes, combustion liners and first-stage turbine blades.
source: usgs-mcs2026-cobalt
where: Domestic Production and Use paragraph
- application: electronics-and-chips
device: Connectors, thermal switches and microsensors in aerospace electronics
example: Wikipedia says cobalt alloys are used in connectors, thermal switches and microsensors that must endure extreme temperatures, vibration and radiation, conditions typical in satellites, fighter aircraft and hypersonic systems.
source: wikipedia-co
where: Alloys section, second paragraph on aerospace-grade electrical components
- application: mechanisms
device: Samarium-cobalt permanent magnets for motors, sensors and aerospace actuators
example: Goodfellow says samarium-cobalt magnets outperform NdFeB above about 150 °C and in corrosive environments, which makes them the choice for high-temperature motors, sensors and aerospace actuators.
source: goodfellow-co-metal
where: Use case table, row Permanent Magnet Research (SmCo)
supply:
- subject: Cobalt mine production, 2025
producers:
- country: Congo (Kinshasa)
share_percent: 73
year: 2025
- country: Indonesia
share_percent: 14
year: 2025
demand: 'USGS mine production in 2025, cobalt content: Congo (Kinshasa) 230,000 t; Indonesia 44,000 t; Russia 7,700 t; Madagascar 3,900 t; Australia 3,700 t; Philippines 3,700 t; Canada 3,500 t; world total 310,000 t (rounded). The printed shares are the estimated share of world total in the Events paragraph.'
source: usgs-mcs2026-cobalt
where: Events, Trends, and Issues paragraph (shares); World Mine Production and Reserves table, column 2025 (tonnes)
- subject: Cobalt reserves and resources
producers: []
demand: 'Reserves: Congo (Kinshasa) 6,000,000 t; Australia 1,700,000 t; Russia 800,000 t; world total 12,000,000 t (rounded). Identified world terrestrial resources are about 25 million tons, mostly in copper deposits of Congo (Kinshasa) and Zambia, nickel laterites, and magmatic nickel-copper sulfides. About 5 billion tons of cobalt is contained in sea floor polymetallic nodules.'
source: usgs-mcs2026-cobalt
where: World Mine Production and Reserves table, Reserves column; World Resources paragraph
- subject: Congo (Kinshasa) export controls
producers: []
demand: Congo (Kinshasa) temporarily banned cobalt exports in February 2025, then replaced the ban with export quotas of 18,125 t of contained cobalt for the rest of 2025 and up to 96,600 t per year in 2026 and 2027, including 9,600 t for national strategic reserves.
source: usgs-mcs2026-cobalt
where: Events, Trends, and Issues paragraph
- subject: United States cobalt use, imports and recycling
producers: []
demand: 'Estimated US use in 2025: superalloys 51 %, chemical applications 25 %, other metallic applications 15 %, cemented carbides 9 %. Apparent consumption 9,600 t in 2025, with net import reliance of 79 % (2025e). Import shares 2021 to 2024: Norway 26 %, Finland 16 %, Canada 14 %, Japan 14 %.'
recycling: Cobalt content of purchased scrap was 25 % of estimated cobalt consumption in 2025 (USGS).
source: usgs-mcs2026-cobalt
where: Domestic Production and Use; Salient Statistics; Import Sources (2021-24); Recycling paragraphs
- subject: Cobalt price, US$ per pound
producers: []
demand: LME cash price averaged 23.17 in 2021, 28.83 in 2022, 15.48 in 2023, 11.84 in 2024 and 15 in 2025 (US$ per pound, USGS). The US spot cathode price averaged 21 in 2025.
source: usgs-mcs2026-cobalt
where: Salient Statistics, Price, average, dollars per pound
- subject: Critical-material status
producers: []
critical_lists:
- list: Described on the Goodfellow page as a critical raw material in the EU and US (list not named)
listed: true
source: goodfellow-co-metal
where: Overview paragraph of the cobalt material page
- subject: Substitutes
producers: []
substitutes:
- 'USGS: cobalt-free lithium-ion cathodes using iron and phosphorus held significant market share in China. In magnets: barium or strontium ferrites, neodymium-iron-boron or nickel-iron alloys. In paints: cerium, iron, lead, manganese or vanadium. In jet engines: nickel-base alloys or ceramics. In cutting and wear-resistant materials: iron, nickel, cermets or ceramics.'
source: usgs-mcs2026-cobalt
where: Substitutes paragraph
documents:
- title: Goodfellow, High-Purity Cobalt Metal, material page
type: datasheet
url: https://www.goodfellow.com/usa/material/metals/cobalt
- title: Goodfellow, High-Purity Cobalt Rod, product page
type: datasheet
url: https://www.goodfellow.com/usa/cobalt-rod-group
- title: Goodfellow, Cobalt Foil 0.025 mm, 99.8 %, technical data sheet (SKU 1000005039)
type: datasheet
url: https://www.goodfellow.com/usa/technical_data/pdf/download?sku=1000005039
- title: 'Wikipedia: Cobalt'
type: database
url: https://en.wikipedia.org/wiki/Cobalt
- title: PubChem compound record for cobalt (CID 104730), with HSDB, ECHA and OSHA entries
type: database
url: https://pubchem.ncbi.nlm.nih.gov/compound/Cobalt
- title: 'USGS Mineral Commodity Summaries 2026: Cobalt'
type: report
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-cobalt.pdf
year: 2026
- title: NIST Atomic Weights and Isotopic Compositions, cobalt
type: database
url: https://physics.nist.gov/cgi-bin/Compositions/stand_alone.pl?ele=Co&all=all&ascii=html
- title: ATSDR Toxic Substances Portal, Cobalt
type: database
url: https://wwwn.cdc.gov/TSP/substances/ToxSubstance.aspx?toxid=64
- title: Fine Metals Corporation, cobalt rod product listing
type: report
url: https://finemetalscorp.com/product/cobalt-rod/
gaps:
- No designation (UNS, EN, AISI, ASTM or trade name) for unalloyed cobalt was printed in any source read in this run. A search for a UNS number returned only cobalt-base alloy standards. Goodfellow's catalogue codes (legacy code CO000190, product code CO00-FL-000290) are supplier codes, not designations, so they are not recorded, and identity.designations is left out.
- 'Yield strength of unalloyed cobalt was not recorded: the Goodfellow table prints 345-485 MPa with no temper, and the rule is to state the temper for each strength value.'
- Vickers hardness, saturation magnetization, latent heat of fusion and the hcp to fcc transformation temperature are not canonical names in spores/property-canon.yaml, so they use the snake_case names vickers_hardness, saturation_magnetization, heat_of_fusion and phase_transformation_temperature.
- Wikipedia prints a density of 8.834 g/cm3 at 20 °C in its infobox, which differs from the 8.90 g/cm3 of the Goodfellow pages and the 8.9 g/cm3 of the rod page. It is not entered, to keep one density per supplier, and the difference is not resolved.
- Atomic-oxygen erosion, outgassing (total mass loss), cold welding and radiation effects on pure cobalt were not found in the sources read. No NASA or ESA test result for cobalt was opened.
- Atmospheric corrosion rate, oxide film thickness and high-temperature oxidation rate for pure cobalt were not found as numbers.
- The Cobalt Institute facts page was fetched but no production, use or supply figure could be read from it, so it is not cited.
- The NIOSH and OSHA chemical-data pages could not be read directly (short error responses), so their limits are taken from the PubChem record, which prints them.
- The critical-mineral status is taken from the Goodfellow page; the USGS summary read here does not name the critical-mineral list.
- Process steps beyond reductive smelting and by-product recovery (refining route, electrowinning) were not read from a primary process source.
- Electrical and thermal properties at cryogenic temperatures were not looked up; the NIST cryogenic tables are not in this profile.
sources:
goodfellow-co-metal:
title: High-Purity Cobalt Metal, Goodfellow material page (Co 99.99 % maximum, 4N), physical, electrical, thermal and mechanical data
id: Goodfellow Metals, cobalt material page
url: https://www.goodfellow.com/usa/material/metals/cobalt
kind: datasheet
license: Supplier web page, cited not reproduced
goodfellow-co-rod:
title: High-Purity Cobalt Rod, Goodfellow product page with material properties for metals
id: Goodfellow Metals, cobalt rod product page
url: https://www.goodfellow.com/usa/cobalt-rod-group
kind: datasheet
license: Supplier web page, cited not reproduced
goodfellow-co-foil:
title: Cobalt Foil/Sheet 0.025 mm x 150 mm x 150 mm, 99.8 % purity, Goodfellow technical data sheet (SKU 1000005039)
id: Goodfellow SKU 1000005039, Product Code CO00-FL-000290
url: https://www.goodfellow.com/usa/technical_data/pdf/download?sku=1000005039
kind: datasheet
license: Supplier data sheet, cited not reproduced
wikipedia-co:
title: Cobalt, Wikipedia (infobox properties, characteristics, alloys and applications)
id: Wikipedia article Cobalt, CC BY-SA 4.0
url: https://en.wikipedia.org/wiki/Cobalt
kind: web
license: CC BY-SA 4.0, linked not reproduced
pubchem-co:
title: PubChem compound record for Cobalt (CID 104730), experimental properties, GHS classification, HSDB and ECHA summaries
id: CID 104730, CAS 7440-48-4, EC 231-158-0
url: https://pubchem.ncbi.nlm.nih.gov/rest/pug_view/data/compound/104730/JSON
kind: database
license: PubChem (NCBI) record; sections attributed to HSDB, ECHA and others
usgs-mcs2026-cobalt:
title: Mineral Commodity Summaries 2026, Cobalt (U.S. Geological Survey, February 2026)
id: USGS MCS 2026, data for 2025
url: https://pubs.usgs.gov/periodicals/mcs2026/mcs2026-cobalt.pdf
year: 2026
kind: report
license: Public domain (USGS)
nist-atomic-weights:
title: NIST Atomic Weights and Isotopic Compositions for All Elements, cobalt row
id: NIST standard atomic weight of Co 58.933 194(4)
url: https://physics.nist.gov/cgi-bin/Compositions/stand_alone.pl?ele=Co&all=all&ascii=html
kind: database
license: US government data
atsdr-cobalt:
title: ATSDR Toxic Substances Portal, Cobalt (CAS 7440-48-4)
id: ATSDR Toxicological profile summary, Cobalt
url: https://wwwn.cdc.gov/TSP/substances/ToxSubstance.aspx?toxid=64
kind: web
license: US government public health information
fine-metals-co-rod:
title: Cobalt Rod, Fine Metals Corporation product listing with specification list
id: Reseller listing, no standard cited
url: https://finemetalscorp.com/product/cobalt-rod/
kind: web
license: Reseller web page, cited not reproduced
license: CC-BY-4.0
updated: '2026-10-26'
review:
status: draft
method: assistant
checked_values: 26
unreachable: 3
caveats: 6
note: 'Values were read by an AI assistant on 2026-10-26 from the pages and PDFs named in each entry. USGS and the Goodfellow foil data sheet were read from PDF text. Unreachable or unhelpful: the NIOSH and OSHA chemical pages returned short error responses, and the Cobalt Institute facts page gave no usable figure. Caveats: supplier values for density and resistivity differ slightly between pages (for example 62.4 nΩ·m and 6.34 µΩ·cm); the Wikipedia density of 8.834 g/cm3 is not entered; the foil values are for one 0.025 mm foil; the 2025 shares of Congo and Indonesia are USGS estimates; the critical-mineral status rests on one supplier page.'
story:
recipe:
line: Cobalt is a single-element metal, Co, with a hexagonal close-packed structure below 417 °C and a face-centred cubic structure above it (Goodfellow). Today it is usually produced as a by-product of copper and nickel mining, and the free element is made by reductive smelting (Wikipedia).
parts:
- name: Cobalt
symbol: Co
atoms: 1
atomic_weight: 58.933194
role: 'The whole material: unalloyed cobalt metal. The NIST standard atomic weight is 58.933 194(4).'
risk_groups:
- title: For people
lead: The EU harmonised classification lists cobalt metal as a skin and respiratory sensitiser, suspected of causing genetic defects, and as a substance that may cause cancer. ECHA notifications differ on the rest.
level: 2
verdict: Carcinogen and sensitiser under EU rules
points:
- label: Harmonised classification
line: 'PubChem prints the EU classification under Regulation (EC) No 1272/2008: H317, H334, H341 and H350, signal word Danger.'
- label: Notifications
line: Of 2,768 company reports to ECHA, one says cobalt does not meet GHS criteria. Among reports that gave codes, H317 is given by more than 99.9 %, H302 by 65.2 % and H330 by 23.4 %.
- title: If it fails
lead: The failure routes printed in the sources are fire from fine powder and acid attack with hydrogen release. No space exposure data for pure cobalt was found.
points:
- label: Fine powder
line: Finely divided cobalt can ignite in air, and dust can form explosive mixtures in air.
- label: Acid
line: Dilute hydrochloric, sulfuric and nitric acids dissolve cobalt, and the reaction releases flammable and explosive hydrogen.
- title: Handling and storage
points:
- label: Dust limits
line: The OSHA limit for cobalt metal dust and fume is 0.1 mg/m3 and the NIOSH limit is 0.05 mg/m3, both as Co.
- label: Keep fine cobalt apart
line: Keep fine cobalt away from air, oxidising agents, acetylene and ammonium nitrate.
why: 'Cobalt is a hard, ferromagnetic metal. Goodfellow gives its density as 8.90 g/cm3 at 20 °C and its melting point as 1495 °C, and it stays ferromagnetic up to its Curie temperature of 1115 °C. Its thermal conductivity is 100 W/(m·K) in the Goodfellow rod data. It is used mainly as an alloy element: superalloys took 51 % of US cobalt use in 2025, mainly for aircraft gas turbine engines (USGS), and the cobalt content of lithium-ion batteries is the leading global use. Congo (Kinshasa) mined an estimated 73 % of world cobalt in 2025.'
uses:
- where: Batteries
line: The cobalt content of lithium-ion batteries is the leading global use of cobalt, according to the USGS. Cobalt-free cells that use iron and phosphorus held a significant share of the market in China.
- where: Aircraft engines
line: In the United States, superalloys took 51 % of cobalt use in 2025, mainly for aircraft gas turbine engines. Goodfellow adds nozzle guide vanes, combustion liners and first-stage turbine blades as cobalt-base alloy parts.
- where: Satellite electronics
line: Wikipedia says cobalt alloys are used in connectors, thermal switches and microsensors that must endure extreme temperatures, vibration and radiation, conditions typical in satellites.
- where: Magnets and actuators
line: Samarium-cobalt magnets outperform NdFeB above about 150 °C and in corrosive environments, which Goodfellow gives as the reason for their use in high-temperature motors, sensors and aerospace actuators.
can_do:
- label: Carry heat
value: 100 W/(m·K)
benchmark: thermal_conductivity
line: The Goodfellow rod data gives 100 W/(m·K) for 0 to 100 °C. A reseller listing gives 1.0 W/(cm·K) at 298.2 K, which is the same order of magnitude.
- label: Stay magnetic when hot
value: 1115 °C Curie temperature
benchmark: curie_temperature
line: Cobalt stops being ferromagnetic only at its Curie temperature of 1115 °C, which Goodfellow describes as the highest of any ferromagnetic element.
- label: Weight
value: 8.90 g/cm3
benchmark: density
line: The density is 8.90 g/cm3 at 20 °C on the Goodfellow metal page, and 8.9 g/cm3 on the rod page.
- label: Melt
value: 1495 °C melting point
benchmark: melting_point
line: The melting point is 1495 °C (1768 K) on the Goodfellow page. PubChem prints the boiling point as 2,927 °C in its HSDB entry, against 2870 °C on the Goodfellow page.
- label: Strength in two tempers (foil)
value: 1135 MPa hard, 760 MPa soft
benchmark: ultimate_tensile_strength
line: A 0.025 mm cobalt foil of 99.8 % purity has tensile strength 1135 MPa in the hard temper and 760 MPa in the soft temper, with Vickers hardness 320 and 170.
- label: Expansion
value: 12.5 ppm/K
benchmark: cte
line: The coefficient of thermal expansion is 12.5 ppm/K from 0 to 100 °C on the Goodfellow rod page, and 12.9 ppm/K at 20 °C in Wikipedia.
compare: Goodfellow describes the density of cobalt as intermediate between those of iron and nickel, and its thermal conductivity as similar to both. Iron and nickel are similar metals, so read the table rows as examples of the same class, not as a ranking.
compare_rows:
- label: Density
benchmark: density
- label: Thermal conductivity
benchmark: thermal_conductivity
- label: Melting point
benchmark: melting_point
handling:
- Specify the temper, since the foil tensile strength is 1135 MPa hard and 760 MPa soft.
- Treat fine powder as pyrophoric, and keep it away from air, acetylene, oxidisers and ammonium nitrate.
- Keep metal dust and fume below 0.1 mg/m3 (OSHA) and 0.05 mg/m3 (NIOSH), both as Co.
good_for:
- 'High-temperature magnets: a Curie temperature of 1115 °C, and samarium-cobalt magnets that outperform NdFeB above about 150 °C (Goodfellow).'
- 'Hot alloys: cobalt-base superalloys for aircraft gas turbine engines (USGS).'
- 'Battery cathodes: the leading global use of cobalt, according to the USGS.'
watch_out:
- 'Supply is concentrated: Congo (Kinshasa) mined an estimated 73 % of world cobalt in 2025, and export quotas run to 96,600 t per year in 2026 and 2027.'
- The EU classification includes H350 (may cause cancer) and H317 (allergic skin reaction).
- Fine powder can ignite in air, and acid attack releases hydrogen.
- No atomic-oxygen, outgassing or radiation data for pure cobalt in space was found.
verdict: Cobalt is a dense, hard, high-temperature ferromagnetic metal with a melting point of 1495 °C and a Curie temperature of 1115 °C. Its main roles are as an alloy element in magnets, superalloys and battery cathodes, and its supply is concentrated in Congo (Kinshasa). The EU classifies the metal as a carcinogen and a sensitiser, and fine powder is pyrophoric. The profile has no space outgassing, atomic-oxygen or designation data for pure cobalt.
References
Every number above carries a reference number. Click one to see the source and where in it the value comes from.